CN105585902A - Waterborne UV curing spraying printing ink and preparation method thereof - Google Patents

Waterborne UV curing spraying printing ink and preparation method thereof Download PDF

Info

Publication number
CN105585902A
CN105585902A CN201610100117.6A CN201610100117A CN105585902A CN 105585902 A CN105585902 A CN 105585902A CN 201610100117 A CN201610100117 A CN 201610100117A CN 105585902 A CN105585902 A CN 105585902A
Authority
CN
China
Prior art keywords
water
parts
solidifies
spraying ink
agent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201610100117.6A
Other languages
Chinese (zh)
Inventor
毛海燕
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Foshan Caigui New Material Co Ltd
Original Assignee
Foshan Caigui New Material Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Foshan Caigui New Material Co Ltd filed Critical Foshan Caigui New Material Co Ltd
Priority to CN201610100117.6A priority Critical patent/CN105585902A/en
Publication of CN105585902A publication Critical patent/CN105585902A/en
Pending legal-status Critical Current

Abstract

The invention discloses waterborne UV curing spraying printing ink and a preparation method thereof and belongs to the technical field of printing ink production. The waterborne UV curing spraying printing ink comprises the following components in parts by weight: 40-60 parts of waterborne epoxy acrylate, 1-4 parts of a water soluble photoinitiator, 15-35 parts of ceramic pigment, 3-8 parts of a cosolvent, 2-20 parts of a hyperdispersant, 0.5-5 parts of a coupling agent and 8-25 parts of water. The waterborne UV curing spraying printing ink disclosed by the invention combines advantages of waterborne and traditional oil-based ink UV photocuring technologies, water is utilized for replacing a reactive diluent in an oily UV curing system, cost is reduced, the problem that the reactive diluent is toxic, irritant and the like is solved, and system viscosity can be regulated more easily.

Description

A kind of water-based UV solidifies spraying ink and preparation method thereof
Technical field
The present invention relates to Printing ink producing technical field, relate in particular to a kind of water-based UV and solidify spraying ink and system thereofPreparation Method.
Background technology
From China in 2009 introduces First ink-jet printer, ceramic ink jet printing technology starts fast at homeHail exhibition. With respect to traditional screen printing and roller printing ceramic printing technology, ceramic ink jet printing technologyRealized contactless unsettled printing, pattern and color are limited by equipment and process no longer, preparation flow letterSingle, prepared product image resolution ratio is high, and third dimension is strong. But in prior art, the pottery that market is generalCeramic ink water is generally solvent type ink, needs, with adding a large amount of organic solvents, to be unfavorable for the health of production operatorAnd contaminated environment, along with the reinforcement gradually of people's environmental consciousness and the gradual perfection of relevant laws and regulations, researchExploitation high-performance, low pollution or even free of contamination ceramic printing technology are the development of ceramic ink jet printing technologyInexorable trend.
Chinese patent application " a kind of UV photocuring ceramic ink jet ink and the side for ceramic surface printing thereofMethod " a kind of UV light-curable ink that is applied to ceramic ink jet technical field disclosed. UV light-curable inkBy UV-irradiation, exciting light initator produces free radical, causes oligomer and reactive diluent crosslinked solidChange into film. It is fast, energy-conservation etc. excellent that traditional oiliness UV curing system has low or VOC free, solidification ratePoint, but skin and the eyes of many reactive diluent compositions to people in its formula have stronger spread effect,Affect the healthy of operator, and price is more expensive.
Summary of the invention
For the deficiencies in the prior art, the invention provides a kind of environment amenable ceramic ink jet printing that is applied toThe water-based UV of technical field solidifies spraying ink:
A kind of water-based UV solidifies spraying ink, it is characterized in that, comprises following parts by weight of component:
Preferably, described water-soluble light trigger is selected from the free radical type water of introducing hydrophily anionic groupDissolubility light trigger, or the free radical type water-soluble light trigger of introducing hydrophily cation group, or introduceThe free radical type water-soluble light trigger of hydrophily non-ionic group.
Further, described hydrophily anionic group is sulfonic group or carboxyl; Described hydrophily cation radicalGroup is quaternary ammonium salt; Described hydrophily non-ionic group is alkoxyl hydroxyl.
Preferably, water-soluble light trigger can be selected from water-based benzoin derivatives, water-based acetophenone derivs,The cracking type light such as water-based alpha-alcohol ketone derivative, water-based α-amido ketone derivatives, water-based acylphosphine oxideInitiator system or water-based benzophenone derivates, water-based thia anthracyclinone derivatives, water-based anthraquinone derivative and workProperty amine combination hydrogen-abstraction light initiation system in one or more.
Preferably, described ceramic pigment is selected from the one in praseodymium zirconium Huang, cobalt blue, reddish brown and cobalt black.
Preferably, described hyper-dispersant is selected from polyacrylate hyper-dispersant; Described coupling agent is selected from siliconOne in alkane coupling agent or titanate coupling agent; Described cosolvent is selected from ethylene glycol, propane diols, isopropylAt least one in alcohol, glycol monoethyl ether, diethylene glycol monomethyl ether, ethylene glycol monobutyl ether.
Further, described water-based UV solidifies spraying ink and also comprises 1~4 part of auxiliary agent, and described auxiliary agent is selected fromIn levelling agent, defoamer, anti-settling agent, bactericide or pH adjusting agent at least two kinds.
Above-mentioned water-based UV solidifies the preparation method of spraying ink, comprises the following steps:
A) prepare mill base: under high-speed stirred, in the mixed liquor of cosolvent and water, add hyper-dispersant, stirHyper-dispersant is fully mixed, slowly add ceramic pigment, high-speed stirred is to mixing;
B) prepare premixed liquid: in the mill base that a) prepared by step, add waterborne epoxy acrylate and coupling agent,Mix, then add auxiliary agent to stir, finally add water-soluble light trigger high-speed stirred, fully mixedClose;
C) prepare ink: premixed liquid is ground to ceramic pigment particle diameter < 1 μ m, obtains water-based UV and solidify sprayInking.
Skin and the eyes of reactive diluent composition in tradition ink UV technology to people have stronger stimulationEffect, affect the healthy of operator, and price is more expensive. Water-based UV of the present invention solidifies spraying inkCombine the advantage of water-based and traditional oil-based ink UV photocuring technology, fortune water consumption substitution oiliness UV solidifiesReactive diluent in system, has reduced cost, has solved the problems such as reactive diluent is toxic, excitant.On the other hand, because reactive diluent has toxicity, must control its use amount, when addition is excessive,The problem of product retrogradation is also relatively difficult to resolve certainly, and with respect to reactive diluent, the viscosity of water is lower, can be veryViscosity and the mobility of good control ink, make ink in the time of printing, show good performance.
Detailed description of the invention
In order to more fully understand technology contents of the present invention, below in conjunction with specific embodiment to technology of the present inventionScheme is further introduced and explanation.
Embodiment 1
By weight, the diethylene glycol monomethyl ether of 5 parts is added in the water of 12 parts, be mixed into diethylene glycol listThe methyl ether aqueous solution; Under high-speed stirred to the polyacrylic acid that adds 11 parts in the aqueous solution of diethylene glycol monomethyl etherEster class hyper-dispersant, stirs hyper-dispersant is fully mixed, and slowly adds the yellow ceramic pigment of praseodymium zirconium of 25 parts,High-speed stirred is mixed with into mill base; To preparation mill base in add 50 parts waterborne epoxy acrylate andThe silane coupler of 2.5 parts, mixes, then adds the levelling agent of 0.5 part, the defoamer, 0.5 of 0.5 partAnti-settling agent, the bactericide of 0.5 part and the pH adjusting agent of 0.5 part of part stir, and finally add 2.5 partsWater-based benzoin derivatives high-speed stirred, be fully mixed with into premixed liquid; Premixed liquid is ground to particle diameter< 1 μ m, obtains water-based UV and solidifies spraying ink.
Embodiment 2
By weight, the ethylene glycol of 3 parts is added in the water of 8 parts, be mixed into glycol water; At heightUnder speed stirs, to the polyacrylate hyper-dispersant that adds 2 parts in glycol water, stir and make oversubscriptionPowder fully mixes, and slowly adds the cobalt blue ceramic pigment of 15 parts, and high-speed stirred is mixed with into mill base; ToIn the mill base of preparation, add the waterborne epoxy acrylate of 40 parts and the titanate coupling agent of 0.5 part, mix allEven, then add the levelling agent of 0.2 part, the defoamer of 0.2 part, the anti-settling agent of 0.2 part, the bactericide of 0.2 partAnd the pH adjusting agent of 0.2 part stirs, finally add the water-based alpha-alcohol ketone derivative of 1 part and 1 partWater-based α-amido ketone derivatives high-speed stirred, be fully mixed with into premixed liquid; Premixed liquid is ground to grainFootpath < 1 μ m, obtains water-based UV and solidifies spraying ink.
Embodiment 3
By weight, the ethylene glycol monobutyl ether of the isopropyl alcohol of 3 parts and 3 parts is added in the water of 25 parts, mixBecome the aqueous solution; Under high-speed stirred, to the polyacrylate hyper-dispersant that adds 20 parts in the aqueous solution, stirHyper-dispersant is fully mixed, slowly add the reddish brown ceramic pigment of 35 parts, high-speed stirred is mixed with intoMill base; In the mill base of preparation, add the waterborne epoxy acrylate of 60 parts and the titanate coupling agent of 5 parts,Mix, then add the levelling agent of 0.8 part, the defoamer of 0.8 part, the anti-settling agent, 0.8 part of 0.8 partThe pH adjusting agent of bactericide and 0.8 part stirs, and finally adds the water-based benzophenone derivates of 4 parts highSpeed stirs, and is fully mixed with into premixed liquid; Premixed liquid is ground to particle diameter < 1 μ m, obtains water-based UVSolidify spraying ink.
Embodiment 4
By weight, the diethylene glycol monomethyl ether of 5 parts is added in the water of 15 parts, be mixed into diethylene glycol listThe methyl ether aqueous solution; Under high-speed stirred to the polyacrylate that adds 8 parts in the diethylene glycol monomethyl ether aqueous solutionClass hyper-dispersant, stirs hyper-dispersant is fully mixed, and slowly adds the cobalt blue ceramic pigment of 20 parts, heightSpeed is uniformly mixed and is prepared into mill base; In the mill base of preparation, add the waterborne epoxy acrylate and 2 of 45 partsThe titanate coupling agent of part, mixes, then adds the levelling agent of 0.4 part, the defoamer, 0.1 of 0.4 partThe anti-settling agent of part and the bactericide of 0.2 part stir, and finally add the water-based acylphosphine oxide of 2 parts highSpeed stirs, and is fully mixed with into premixed liquid; Premixed liquid is ground to particle diameter < 1 μ m, obtains water-based UVSolidify spraying ink.
Embodiment 5
By weight, the isopropyl alcohol of 6 parts is added in the water of 20 parts, be mixed into isopropanol water solution; At heightUnder speed stirs, to the polyacrylate hyper-dispersant that adds 2 parts in isopropanol water solution, stir and make oversubscriptionPowder fully mixes, and slowly adds the cobalt black ceramic pigment of 25 parts, and high-speed stirred is mixed with into mill base; ToIn the mill base of preparation, add the waterborne epoxy acrylate of 55 parts and the silane coupler of 4.5 parts, mix,Add again the levelling agent of 0.1 part, the defoamer of 0.2 part, the anti-settling agent of 0.3 part, the bactericide and 0.5 of 0.4 partThe pH adjusting agent of part stirs, and finally adds the water-based acetophenone derivs of 1.5 parts and the water-based of 1.5 partsThioxanthone derivative high-speed stirred, is fully mixed with into premixed liquid; Premixed liquid is ground to particle diameter < 1μ m, obtains water-based UV and solidifies spraying ink.
Embodiment 6
By weight, the isopropyl alcohol of 3 parts is added in the water of 8 parts, be mixed into isopropanol water solution; At heightUnder speed stirs, to the polyacrylate hyper-dispersant that adds 2 parts in isopropanol water solution, stir and make oversubscriptionPowder fully mixes, and slowly adds the cobalt blue ceramic pigment of 15 parts, and high-speed stirred is mixed with into mill base; ToIn the mill base of preparation, add the waterborne epoxy acrylate of 40 parts and the titanate coupling agent of 0.5 part, mix allEven, then add the levelling agent of 0.2 part, the defoamer of 0.1 part, the anti-settling agent of 0.3 part, the bactericide of 0.2 partAnd the pH adjusting agent of 0.2 part stirs, finally add the water-based alpha-alcohol ketone derivative of 3 parts and 1 partWater-based α-amido ketone derivatives high-speed stirred, be fully mixed with into premixed liquid; Premixed liquid is ground to grainFootpath < 1 μ m, obtains water-based UV and solidifies spraying ink.
Embodiment 7
By weight, the ethylene glycol of 3 parts is added in the water of 8 parts, be mixed into glycol water; At heightUnder speed stirs, to the polyacrylate hyper-dispersant that adds 2 parts in glycol water, stir and make oversubscriptionPowder fully mixes, and slowly adds the cobalt blue ceramic pigment of 15 parts, and high-speed stirred is mixed with into mill base; ToIn the mill base of preparation, add the waterborne epoxy acrylate of 40 parts and the titanate coupling agent of 0.5 part, mix allEven, then add the levelling agent of 0.2 part, the defoamer of 0.2 part, the anti-settling agent of 0.2 part, the bactericide of 0.2 partAnd the pH adjusting agent of 0.2 part stirs, finally add the water-based anthraquinone derivative hydrogen-abstraction of 3 parts light-initiatedAgent and reactive amines are pressed the mixture high-speed stirred of 1:1 combination, are fully mixed with into premixed liquid; By premixed liquidBe ground to particle diameter < 1 μ m, obtain water-based UV and solidify spraying ink.
Embodiment 8
By weight, the isopropyl alcohol of 3 parts is added in the water of 8 parts, be mixed into isopropanol water solution; At heightUnder speed stirs, to the polyacrylate hyper-dispersant that adds 2 parts in isopropanol water solution, stir and make oversubscriptionPowder fully mixes, and slowly adds the cobalt blue ceramic pigment of 15 parts, and high-speed stirred is mixed with into mill base; ToIn the mill base of preparation, add the waterborne epoxy acrylate of 40 parts and the titanate coupling agent of 0.5 part, mix allEven, then add the levelling agent of 0.1 part, the defoamer of 0.2 part, the anti-settling agent of 0.3 part, the bactericide of 0.4 partAnd the pH adjusting agent of 0.5 part stirs, finally add the water-based anthraquinone derivative hydrogen-abstraction of 3 parts light-initiatedAgent and reactive amines are pressed the mixture of 1:1 combination, are fully mixed with into premixed liquid; Premixed liquid is ground to grainFootpath < 1 μ m, obtains water-based UV and solidifies spraying ink.
Embodiment 9
By weight, the ethylene glycol monobutyl ether of the isopropyl alcohol of 3 parts and 3 parts is added in the water of 25 parts, mixBecome the aqueous solution; Under high-speed stirred, to the polyacrylate hyper-dispersant that adds 20 parts in the aqueous solution, stirHyper-dispersant is fully mixed, slowly add the reddish brown ceramic pigment of 35 parts, high-speed stirred is mixed with intoMill base; In the mill base of preparation, add the waterborne epoxy acrylate of 60 parts and the titanate coupling agent of 5 parts,Mix, then add the levelling agent of 0.8 part, the defoamer of 0.8 part, the anti-settling agent, 0.8 part of 0.8 partThe pH adjusting agent of bactericide and 0.8 part stirs, finally add 4 parts water-based benzophenone derivates withWater-based alpha-alcohol ketone derivative is pressed the mixture high-speed stirred of 1:1 combination, is fully mixed with into premixed liquid;Premixed liquid is ground to particle diameter < 1 μ m, obtains water-based UV and solidify spraying ink.
Embodiment 10
By weight, the ethylene glycol of 2 parts is added in the water of 15 parts, be mixed into glycol water; At heightUnder speed stirs, to the polyacrylate hyper-dispersant that adds 15 parts in glycol water, stir and make oversubscriptionPowder fully mixes, and slowly adds the reddish brown ceramic pigment of 15 parts, and high-speed stirred is mixed with into mill base; ToIn the mill base of preparation, add the waterborne epoxy acrylate of 40 parts and the silane coupler of 0.5 part, mix,Add again the levelling agent of 0.6 part, the defoamer of 0.6 part, the anti-settling agent of 0.6 part, the bactericide and 0.6 of 0.6 partThe pH adjusting agent of part stirs, and finally adds the water-based alpha-alcohol ketone derivative of 1 part and the water-based of 1 partα-amido ketone derivatives high-speed stirred, is fully mixed with into premixed liquid; Premixed liquid is ground to particle diameter < 1μ m, obtains water-based UV and solidifies spraying ink.
The above only further illustrates technology contents of the present invention with embodiment, so that reader is easierUnderstand, but do not represent that embodiments of the present invention only limit to this, any technology of doing according to the present invention extend orRecreation, is all subject to protection of the present invention.

Claims (10)

1. water-based UV solidifies a spraying ink, it is characterized in that, comprises following parts by weight of component:
2. water-based UV according to claim 1 solidifies spraying ink, it is characterized in that described waterDissolubility light trigger is selected from the free radical type water-soluble light trigger of introducing hydrophily anionic group, or introducesThe free radical type water-soluble light trigger of hydrophily cation group, or introduce hydrophily non-ionic group fromBy fundamental mode water-soluble light trigger.
3. water-based UV according to claim 2 solidifies spraying ink, it is characterized in that, described hydrophilicProperty anionic group is sulfonic group or carboxyl; Described hydrophily cation group is quaternary ammonium salt.
4. water-based UV according to claim 2 solidifies spraying ink, it is characterized in that described parentWater-based non-ionic group is alkoxyl hydroxyl.
5. water-based UV according to claim 1 solidifies spraying ink, it is characterized in that described potteryPorcelain color is selected from the one in praseodymium zirconium Huang, cobalt blue, reddish brown and cobalt black.
6. water-based UV according to claim 1 solidifies spraying ink, it is characterized in that described oversubscriptionPowder is selected from polyacrylate hyper-dispersant.
7. water-based UV according to claim 1 solidifies spraying ink, it is characterized in that described idolConnection agent is selected from the one in silane coupler or titanate coupling agent.
8. water-based UV according to claim 1 solidifies spraying ink, it is characterized in that, described helpsSolvent is selected from ethylene glycol, propane diols, isopropyl alcohol, glycol monoethyl ether, diethylene glycol monomethyl ether, ethylene glycolAt least one in monobutyl ether.
9. solidify spraying ink according to the water-based UV described in claim 1-8 any one, it is characterized in that,Also comprise 1~4 part of auxiliary agent, described auxiliary agent is selected from levelling agent, defoamer, anti-settling agent, bactericide or pH and adjustsSave at least two kinds in agent.
10. the preparation method that water-based UV solidifies spraying ink as claimed in claim 9, is characterized in that, bagDraw together following steps:
A) prepare mill base: under high-speed stirred, in the mixed liquor of cosolvent and water, add hyper-dispersant, stirHyper-dispersant is fully mixed, slowly add ceramic pigment, high-speed stirred is to mixing;
B) prepare premixed liquid: in the mill base that a) prepared by step, add waterborne epoxy acrylate and coupling agent,Mix, then add auxiliary agent to stir, finally add water-soluble light trigger high-speed stirred, fully mixedClose;
C) prepare ink: premixed liquid is ground to ceramic pigment particle diameter < 1 μ m, obtains water-based UV and solidify sprayInking.
CN201610100117.6A 2016-02-23 2016-02-23 Waterborne UV curing spraying printing ink and preparation method thereof Pending CN105585902A (en)