CN108411163A - 一种高强度的γ′相强化型钴基高温合金 - Google Patents
一种高强度的γ′相强化型钴基高温合金 Download PDFInfo
- Publication number
- CN108411163A CN108411163A CN201810211978.0A CN201810211978A CN108411163A CN 108411163 A CN108411163 A CN 108411163A CN 201810211978 A CN201810211978 A CN 201810211978A CN 108411163 A CN108411163 A CN 108411163A
- Authority
- CN
- China
- Prior art keywords
- alloy
- phase
- cobalt
- strength
- temperature
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明公开了一种高强度的γ′相强化型钴基高温合金,该合金材料主要由Co、Ni、Al、W、Cr、Ta、Ti等元素组成,其质量百分比表示为:20.0‑24.5%Ni,14.5‑19.5%W,3.4‑6.0%Al,3.0‑6.8%Cr,4.0‑5.8%Ta,1.5‑2.0%Ti,0.3‑1.0%Mo,0‑0.14%Zr,0.01‑0.015%B,0‑0.1%C,0‑0.007%Y,Co为余量。该合金的主要组成相是(a)钴基固溶体γ+金属间化合物γ′,或(b)钴基固溶体γ+金属间化合物γ′+MC型碳化物+晶界弥散析出金属间化合物μ。该合金可用于冶金、石油、能源、电力等工业领域中涡轮机热端部件,其工作温度可达900℃。该合金高温强度较高,高温条件下(700‑900℃)该合金的屈服强度约为DZ40M的2‑3倍;该合金的持久性能、抗高温氧化和热腐蚀性能优异,均优于传统钴基高温合金。
Description
技术领域
本发明属于新材料技术领域,涉及一种高强度的新型γ′相强化型钴基高温合金。
背景技术
提高燃气轮机的功率和效率,提升燃气入口温度(Turbine Inlet Temperature,TIT)是促进现代工业发展的重要前提。而燃气轮机TIT的提高须靠综合性能优异的高温合金来保证。目前,国内外广泛使用镍基高温合金(如IN738LC、Rene5SC、MGA1400,GTD-111DS等)作为燃气轮机热端部件材料。与镍基高温合金相比,钴基高温合金虽然具有抗蠕变性能和抗热腐蚀性能好、低热膨胀系数以及高导热性等优点,但是传统钴基高温合金缺乏γ′相沉淀强化效应,其高温强度无法得到保证,仅在燃气轮机中导向叶片等低应力需求的场合中有所应用。
自2006年Sato.等在Co-Al-W合金中发现了具有L12结构γ′-Co3(Al,W),其强化方式与传统的镍基高温合金相似,有望大幅度提高钴基合金的高温强度。不仅如此,钴基高温合金的初溶温度高于镍基高温合金,可打破熔点给高温合金使用温度的提升带来的制约。资料显示,燃气轮机TIT每提升10℃,其功率和效率可提高1%,因此新型γ′相强化钴基高温合金的研发具有很大的应用前景。
新型钴基高温合金的研发初期,有研究学者指出,900和1000℃时Sato.等所发现的γ′相相区非常小,并处于一种亚稳的状态,900℃时γ′相容易向γ、D019和B2相转化。因此Ta、Ti、Nb、Mo和V等元素需要添加到钴基合金中以稳定γ′相。然而Ta、Mo添加可促进μ相析出,Ti可促进形成Co2AlTi,而V、Nb等能够显著降低合金的抗氧化性能。添加合金元素的同时,需要综合考虑各元素对合金相平衡、力学行为和抗高温氧化及热腐蚀行为的影响。因此,优化合金成分设计成为了新型钴基高温合金研发的关键。
发明内容
本发明目的旨在提供一种具有较高的高温强度、良好的持久性能、优异的抗高温氧化和抗热腐蚀性能的新材料。其γ′相可在950℃以下稳定存在并为立方形貌,且该相体积百分数可达60%以上。
本发明合金的成分特点考虑了如下因素:
Ni:稳定γ基体,并扩大γ′相相区,增加合金γ′相的初溶温度。
W:γ′相的组成元素,且W含量越高,γ′相的初溶温度越高。不仅如此,W固溶于基体中起到固溶强化作用,使合金具有更高的高温强度。
Al:γ′相的组成元素,且在高温氧化和热腐蚀过程中,合金表面形成氧化铝层,可保护基体被进一步氧化或腐蚀,然而Al含量较高合金将析出β相。
Ti:Ti在γ′相中倾向于占Co/W位,Ti稳定γ′相(增加其析出温度和体积分数),Ti和Ta结合可显著提升抗氧化性和蠕变性能,然而Ti含量较高合金将析出β相。
Ta:Ta在γ′相中倾向于占W位,Ta稳定γ′相(增加其析出温度和体积分数),然而Ta含量较高合金将球化γ′相。
Cr:Cr在γ′相中倾向于占Co/W位,降低γ′相的析出温度和体积分数,Cr添加量高于8%时,γ′相将球化;Cr的添加可增加合金的氧化性能,但在950℃以上的氧化中其作用显著降低。
Mo:Mo在γ′相中倾向于中占W位,Mo稳定γ′相(降低其析出温度和增加体积分数),然而W、Ta和Mo总添加量不宜过高,易析出χ相和μ相。
Zr:减少晶界缺陷,提高晶界结合力,强化晶界。
B:增加晶界结合力,提高合金的抗氧化性、蠕变性能和持久性能。
C:晶界强化元素,提高合金高温持久寿命。
Y:增加合金抗氧化性能。
本发明的技术方案是:一种高强度的γ′相强化型钴基高温合金,该合金成分按重量计:20.0-24.5%Ni,14.5-19.5%W,3.4-6.0%Al,3.0-6.8%Cr,4.0-5.8%Ta,1.5-2.0%Ti,0.3-1.0%Mo,0-0.14%Zr,0.01-0.015%B,0-0.1%C,0-0.007%Y,Co为余量。
进一步地,上述钴基高温合金中相应成分按重量计:14.5-15.5%W,3.6-4.3%Al,5.8-6.8%Cr,5.4-5.8%Ta,1.5-1.8%Ti,0.3-0.5%Mo,0-0.02%C。该合金的特征铬含量较高,主要组成相为钴基固溶体γ+金属间化合物γ′,合金抗氧化性能优异。
进一步地,上述钴基高温合金中相应成分按重量计:15.0-19.5%W,3.6-4.3%Al,5.8-6.8%Cr,5.4-5.8%Ta,1.5-1.8%Ti,0.3-0.5%Mo,0.02-0.1%C。该合金的特征铬、碳含量较高,主要组成相为钴基固溶体γ+金属间化合物γ′+MC型碳化物+晶界弥散析出金属间化合物μ,该合金抗氧化性能优异,晶界存在碳化物等,提高了合金的高温持久、蠕变等性能。
进一步地,上述钴基高温合金中相应成分按重量计:14.0-16.0%W,3.8-4.3%Al,3.0-4.0%Cr,5.0-5.8%Ta,1.5-1.8%Ti,0-0.02%C。该合金的特征铬含量较低,钨含量增加,主要组成相为钴基固溶体γ+金属间化合物γ′,该合金固溶强化元素含量较高,可具有更高高温强度。
进一步地,上述钴基高温合金中相应成分按重量计:15.0-19.5%W,3.8-4.2%Al,3.0-5.0%Cr,5-5.8%Ta,1.5-1.8%Ti,0.02-0.1%C。该合金的特征碳含量较高,铬含量较低,钨含量增加,主要组成相为钴基固溶体γ+金属间化合物γ′+MC型碳化物+晶界弥散析出金属间化合物μ,该合金固溶强化元素含量较高,可具有更高高温强度,且晶界存在碳化物等,提高了合金的高温持久、蠕变等性能。
上述高强度的γ′相强化型钴基高温合金的应用,将高强度的γ′相强化型钴基高温合金用于制造燃气轮机热端部件,应用环境温度为800-950℃。
本发明的有益效果为,发明合金的高温强度较高,高温屈服强度约为传统钴基定向凝固高温合金DZ40M的2.5-3倍;发明合金的高温抗氧化性能优异,900℃条件下,平均氧化速率相比于传统钴基定向凝固高温合金DZ40M减少了约65%-75%;发明合金的高温抗腐蚀性能优异,900℃条件下,平均腐蚀速率相比于传统钴基定向凝固高温合金DZ40M减少了约55%-75%。一种新型γ′相强化型钴基高温合金材料。新材料通过γ′相强化,合金的高温强度较高,且持久性能、抗高温氧化性能和热腐蚀性能优异。
附图说明
图1为本发明(合金2)1220℃固溶8h,950℃时效100h后的γ+γ′组织形貌
图2为实施例合金和比较例合金高温条件下的屈服强度(DZ40M数据来源于《中国高温合金手册》)
具体实施方案
下面对本发明的较佳实施例进行做详细描述。
本发明提供了多组实施例,其化学成分如表1所示。合金具有优良的γ+γ′两相组织。图1为合金3经1220℃固溶8h,950℃时效100h后的组织形貌,显示γ′相为立方形貌,γ′相体积百分数约为70%。说明本发明合金在高温条件下应具有较高的高温强度,具有优异的承温性能。
表1为实施例和比较例的化学成分(按重量百分数计)
DZ40M中含0.95%Fe,0.6%Si和0.44%Mn。
实施例1
表1中,合金1的屈服强度较高,由图2可知,合金1的屈服强度约为传统钴基定向凝固高温合金DZ40M的2.5倍。不仅如此,合金1具有良好的抗高温氧化性能和抗热腐蚀性能。表2为900℃条件下合金1-3和DZ40M的平均氧化速率并根据标准名称《钢及高温合金的抗氧化性测定试验方法》(标准号HB5258-2000,实施日期2001年1月1日)对合金抗氧化性能评定;表3为800、900℃条件下合金1-3的平均热腐蚀增重。由表2和表3可知,实施例合金1与DZ40M相比,平均氧化增重和平均热腐蚀增重均显著小于比较例合金,表现出优异的抗氧化性能和抗热腐蚀性能。
表2 900℃条件下合金1-3和DZ40M的平均氧化速率及合金抗氧化性能评定
合金 | 平均氧化增重g/(m2·h) | 抗氧化性能评定 |
合金1 | 0.03151 | 完全抗氧化级 |
合金2 | 0.02222 | 完全抗氧化级 |
合金3 | 0.02529 | 完全抗氧化级 |
DZ40M | 0.08844 | 完全抗氧化级 |
表3 800、900℃条件下合金1-3的平均热腐蚀增重
(DZ40M数据来源于《中国高温合金手册》)
实施例2
表1中,合金2的屈服强度较高,由图2可知,合金2的高温屈服强度约为传统钴基定向凝固高温合金DZ40M的2.5-3倍。不仅如此,由表2和表3可知,实施例合金2与DZ40M相比,平均氧化增重和平均热腐蚀增重均显著小于比较例合金,表现出优异的抗氧化性能和抗热腐蚀性能。
实施例3
表1中,合金3的屈服强度较高,由图2可知,合金3的高温屈服强度约为传统钴基定向凝固高温合金DZ40M的2.5-3倍。不仅如此,由表2和表3可知,实施例合金3与DZ40M相比,平均氧化增重和平均热腐蚀增重均显著小于比较例合金,表现出优异的抗氧化性能和抗热腐蚀性能。此外,实施例合金3具有良好的持久性能。温度为900℃,试验应力为160MPa条件下实施例合金3的持久寿命高达184.117h,而DZ40M为85h。本发明合金表现出优异的高温持久性能。(DZ40M数据来源于《中国高温合金手册》)
Claims (9)
1.一种高强度的γ′相强化型钴基高温合金,其特征在于,该合金成分按重量计:20.0-24.5%Ni,14.5-19.5%W,3.4-6.0%Al,3.0-6.8%Cr,4.0-5.8%Ta,1.5-2.0%Ti,0.3-1.0%Mo,0-0.14%Zr,0.01-0.015%B,0-0.1%C,0-0.007%Y,Co为余量。
2.根据权利要求1所述的高强度的γ′相强化型钴基高温合金,其特征在于,按重量计:14.5-15.5%W,3.6-4.3%Al,5.8-6.8%Cr,5.4-5.8%Ta,1.5-1.8%Ti,0.3-0.5%Mo,0-0.02%C。
3.根据权利要求1所述的高强度的γ′相强化型钴基高温合金,其特征在于,按重量计:15.0-19.5%W,3.6-4.3%Al,5.8-6.8%Cr,5.4-5.8%Ta,1.5-1.8%Ti,0.3-0.5%Mo,0.02-0.1%C。
4.根据权利要求1所述的高强度的γ′相强化型钴基高温合金,其特征在于,按重量计:14.0-16.0%W,3.8-4.3%Al,3.0-4.0%Cr,5.0-5.8%Ta,1.5-1.8%Ti,0-0.02%C。
5.根据权利要求1所述的高强度的γ′相强化型钴基高温合金,其特征在于,按重量计:15.0-19.5%W,3.8-4.2%Al,3.0-5.0%Cr,5-5.8%Ta,1.5-1.8%Ti,0.02-0.1%C。
6.根据权利要求1所述的高强度的γ′相强化型钴基高温合金,其特征在于,该合金成分按重量计:21.32%Ni,19.47%W,3.47%Al,6.30%Cr,4.11%Ta,1.81%Ti,0.73%Mo,0.14%Zr,0.013%B,0.006%Y,Co为余量。
7.根据权利要求1所述的高强度的γ′相强化型钴基高温合金,其特征在于,该合金成分按重量计:23.87%Ni,14.38%W,3.80%Al,6.51%Cr,5.66%Ta,1.87%Ti,0.30%Mo,0.14%Zr,0.014%B,0.007%Y,Co为余量。
8.根据权利要求1所述的高强度的γ′相强化型钴基高温合金,其特征在于,该合金成分按重量计:23.87%Ni,15.72%W,3.80%Al,6.51%Cr,5.66%Ta,1.87%Ti,0.30%Mo,0.14%Zr,0.014%B,0.007%Y,0.09%C,Co为余量。
9.权利要求1-8任一所述高强度的γ′相强化型钴基高温合金的应用,其特征在于,将高强度的γ′相强化型钴基高温合金用于制造燃气轮机热端部件,应用环境温度为800-950℃。