[go: up one dir, main page]

CN103788911B - Environment-friendly adhesive containing modified nanometer bamboo charcoal powder - Google Patents

Environment-friendly adhesive containing modified nanometer bamboo charcoal powder Download PDF

Info

Publication number
CN103788911B
CN103788911B CN201410057025.5A CN201410057025A CN103788911B CN 103788911 B CN103788911 B CN 103788911B CN 201410057025 A CN201410057025 A CN 201410057025A CN 103788911 B CN103788911 B CN 103788911B
Authority
CN
China
Prior art keywords
parts
bamboo charcoal
environment
charcoal powder
powder
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201410057025.5A
Other languages
Chinese (zh)
Other versions
CN103788911A (en
Inventor
何益庆
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Zhaoping Science Technology Guidance Station
Original Assignee
Tongling Xiangyun Fire Fighting Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tongling Xiangyun Fire Fighting Technology Co Ltd filed Critical Tongling Xiangyun Fire Fighting Technology Co Ltd
Priority to CN201410057025.5A priority Critical patent/CN103788911B/en
Publication of CN103788911A publication Critical patent/CN103788911A/en
Application granted granted Critical
Publication of CN103788911B publication Critical patent/CN103788911B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses an environment-friendly adhesive containing modified nanometer bamboo charcoal powder. The environment-friendly adhesive comprises the following components in parts by weight: 100-150 parts of polyvinyl alcohol resin, 50-80 parts of 2-ethylbenzofuran, 20-30 parts of dibutyl phthalate, 15-20 parts of polystyrene, 10-15 parts of ditolyl phosphate ester, 20-30 parts of isophorone diisocyanate, 5-10 parts of nitrile rubber, 10-15 parts of calcium carbonate, 5-8 parts of titanium dioxide, 5-20 parts of nanometer magnesium hydrate, 15-20 parts of modified nanometer bamboo charcoal powder, 10-15 parts of lignin, 3-5 parts of fused silica, 3-5 parts of sodium alginate, 20-30 parts of quartz sand, 1-3 parts of boron powder, 5-10 parts of windshield washer fluid, 0.7-0.9 parts of dibutyltin dilaurate, 2-4 parts of mica iron oxide, 1-3 parts of silane coupling agent and 10-15 parts of modified fly ash. The adhesive disclosed by the invention has the characteristics of high adhesive strength, no pollution, long storage life and the like, and is harmless to a human body, and environment-friendly.

Description

A kind of environment-protective adhesive containing modified Nano bamboo charcoal powder
Technology neighborhood
The present invention relates to sizing agent technology neighborhood, particularly relate to a kind of environment-protective adhesive containing modified Nano bamboo charcoal powder.
Background technology
Sizing agent is a kind of material that similar or inhomogeneous material tight can be combined.Along with development that is scientific and technical and national economy, tackiness agent has been widely used in every profession and trade and the high-tech neighborhoods such as wood working, construction work, textile printing and dyeing, shoemaking, leather, electronics, automobile, machinery, aerospace, biologic medical.
At present, in order to improve some performance of tackiness agent, add some properties-correcting agent, thickening material, tackifier, emulsifying agent etc., and in these materials, some is poisonous in sizing agent of being everlasting, some or even extremely poison, and majority can produce environmental pollution.
Summary of the invention
The object of the invention is to overcome the deficiencies in the prior art, provide a kind of and have that water-tolerant, bonding strength are high, environmentally safe, environmental protection harmless to human body the sizing agent containing modified Nano bamboo charcoal powder.
The present invention adopts following technical scheme to achieve these goals:
A kind of environment-protective adhesive containing modified Nano bamboo charcoal powder, comprise the component of following weight part: polyvinyl alcohol resin 100-150 part, 2-ethyl benzofuran 50-80 part, dibutyl phthalate 20-30 part, polystyrene 15-20 part, dixylenyl phosphate 10-15 part, isophorone diisocyanate 20-30 part, paracril 5-10 part, calcium carbonate 10-15 part, titanium dioxide 5-8 part, nano-sized magnesium hydroxide 5-20 part, modified Nano bamboo charcoal powder 15-20 part, xylogen 10-15 part, gas-phase silica 3-5 part, sodium alginate 3-5 part, quartz sand 20-30 part, boron powder 1-3 part, bath of glass 5-10 part, dibutyl tin laurate 0.7-0.9 part, iron mica 2-4 part, silane coupling agent 1-3 part, modified coal ash 10-15 part.
The preparation method of described modified Nano bamboo charcoal powder is: bamboo charcoal powder 10-15% sodium hydroxide solution soaks 5-8h, then deionized water wash is used, dry, add again and be equivalent to 2,4 of its weight 1-2%, the ethyl α-cyanoacrylate of 6 trisphenols, 1-3%, the crosslink agent DCP of 1-3%, 3000-5000 rev/min is stirred 30-50 minute, dry, grind to form nanometer powder.
Described modified coal ash is prepared by following steps: first dried in 100-110 DEG C of baking oven by flyash, then the flyash after oven dry is put into high-speed kneading machine, add be equivalent to flyash weight 3-5% aluminate coupling agent, the wooden sodium sulfonate of 2-4%, the triethyl citrate of 2-4%, the whiteruss of 1-2% and 2-5% talcum powder, after high-speed mixing, dry, pulverize and grind to form ultrafine powder.
The preparation method of the described environment-protective adhesive containing modified Nano bamboo charcoal powder, comprises following preparation process:
(1) by recipe ratio, just polyvinyl alcohol resin, 2-ethyl benzofuran, dibutyl phthalate, polystyrene, dixylenyl phosphate, isophorone diisocyanate, paracril, dibutyl tin laurate join reactor and are heated to 100-130 DEG C, high-speed stirring 3-4h;
(2) again other compositions are joined in the reactor in step (1), stir 1-2h, be cooled to normal temperature, pack.
Compared with the prior art, beneficial effect of the present invention is as follows:
The present invention is by adding the compositions such as modified Nano bamboo charcoal powder, xylogen in sizing agent, effectively can eliminate toxicity and the pollution on the environment of sizing agent, simultaneously, add modified coal ash, significantly improve the dispersing uniformity of each component, the adhesion intensity of sizing agent can be improved, and have that cost is low, the feature of excellent effect.Sizing agent of the present invention has the features such as bonding strength is high, pollution-free, storage period is longer, harmless to human body, environmental protection.
Embodiment
Below in conjunction with embodiment, the invention will be further described.
Embodiment 1:
A kind of environment-protective adhesive containing modified Nano bamboo charcoal powder, comprise the component of following weight part: polyvinyl alcohol resin 130 parts, 2-ethyl benzofuran 70 parts, dibutyl phthalate 20 parts, polystyrene 15 parts, dixylenyl phosphate 13 parts, isophorone diisocyanate 25 parts, paracril 7 parts, 10 parts, calcium carbonate, titanium dioxide 5 parts, nano-sized magnesium hydroxide 6 parts, modified Nano bamboo charcoal powder 18 parts, 15 parts, xylogen, gas-phase silica 4 parts, sodium alginate 4 parts, quartz sand 25 parts, 2 parts, boron powder, bath of glass 6 parts, dibutyl tin laurate 0.8 part, iron mica 3 parts, silane coupling agent 2 parts, modified coal ash 13 parts.
Wherein, the preparation method of modified Nano bamboo charcoal powder is: bamboo charcoal powder 15% sodium hydroxide solution soaks 8h, then use deionized water wash, dry, then add and be equivalent to 2 of its weight 2%, 4,6 trisphenols, the ethyl α-cyanoacrylate of 3%, the crosslink agent DCP of 3%, 5000 revs/min are stirred 50 minutes, dry, grind to form nanometer powder.
Modified coal ash is prepared by following steps: first dried in 110 DEG C of baking ovens by flyash, then the flyash after oven dry is put into high-speed kneading machine, add be equivalent to flyash weight 5% aluminate coupling agent, 3% wooden sodium sulfonate, the triethyl citrate of 3%, the whiteruss of 2% and 4% talcum powder, after high-speed mixing, dry, pulverize and grind to form ultrafine powder.
The preparation method of the environment-protective adhesive containing modified Nano bamboo charcoal powder, comprises following preparation process:
(1) by recipe ratio, just polyvinyl alcohol resin, 2-ethyl benzofuran, dibutyl phthalate, polystyrene, dixylenyl phosphate, isophorone diisocyanate, paracril, dibutyl tin laurate join reactor and are heated to 130 DEG C, high-speed stirring 3h;
(2) again other compositions are joined in the reactor in step (1), stir 1h, be cooled to normal temperature, pack.
Embodiment 2:
A kind of environment-protective adhesive containing modified Nano bamboo charcoal powder, comprise the component of following weight part: polyvinyl alcohol resin 100 parts, 2-ethyl benzofuran 50 parts, dibutyl phthalate 20 parts, polystyrene 15 parts, dixylenyl phosphate 10 parts, isophorone diisocyanate 20 parts, paracril 5 parts, 10 parts, calcium carbonate, titanium dioxide 7 parts, nano-sized magnesium hydroxide 5, part, modified Nano bamboo charcoal powder 15 parts, 10 parts, xylogen, gas-phase silica 3 parts, sodium alginate 3 parts, quartz sand 20 parts, 1 part, boron powder, bath of glass 5 parts, dibutyl tin laurate 0.7 part, iron mica 2 parts, silane coupling agent 2 parts, modified coal ash 10 parts.
Wherein, the preparation method of modified Nano bamboo charcoal powder is: bamboo charcoal powder 10% sodium hydroxide solution soaks 7h, then use deionized water wash, dry, then add and be equivalent to 2 of its weight 2%, 4,6 trisphenols, the ethyl α-cyanoacrylate of 1%, the crosslink agent DCP of 1%, 3000 revs/min are stirred 30 minutes, dry, grind to form nanometer powder.
Modified coal ash is prepared by following steps: first dried in 100 DEG C of baking ovens by flyash, then the flyash after oven dry is put into high-speed kneading machine, add be equivalent to flyash weight 3% aluminate coupling agent, 2% wooden sodium sulfonate, the triethyl citrate of 2%, the whiteruss of 1% and 2% talcum powder, after high-speed mixing, dry, pulverize and grind to form ultrafine powder.
The preparation method of the environment-protective adhesive containing modified Nano bamboo charcoal powder, comprises following preparation process:
(1) by recipe ratio, just polyvinyl alcohol resin, 2-ethyl benzofuran, dibutyl phthalate, polystyrene, dixylenyl phosphate, isophorone diisocyanate, paracril, dibutyl tin laurate join reactor and are heated to 100 DEG C, high-speed stirring 3h;
(2) again other compositions are joined in the reactor in step (1), stir 1h, be cooled to normal temperature, pack.
Embodiment 3:
A kind of environment-protective adhesive containing modified Nano bamboo charcoal powder, comprise the component of following weight part: polyvinyl alcohol resin 150 parts, 2-ethyl benzofuran 80 parts, dibutyl phthalate 30 parts, polystyrene 20 parts, dixylenyl phosphate 15 parts, isophorone diisocyanate 30 parts, paracril 10 parts, 15 parts, calcium carbonate, titanium dioxide 8 parts, nano-sized magnesium hydroxide 20 parts, modified Nano bamboo charcoal powder 20 parts, 15 parts, xylogen, gas-phase silica 5 parts, sodium alginate 5 parts, quartz sand 30 parts, 3 parts, boron powder, bath of glass 8 parts, dibutyl tin laurate 0.9 part, iron mica 4 parts, silane coupling agent 3 parts, modified coal ash 15 parts.
Wherein, the preparation method of modified Nano bamboo charcoal powder is: bamboo charcoal powder 15% sodium hydroxide solution soaks 5h, then use deionized water wash, dry, then add and be equivalent to 2 of its weight 2%, 4,6 trisphenols, the ethyl α-cyanoacrylate of 3%, the crosslink agent DCP of 3%, 5000 revs/min are stirred 50 minutes, dry, grind to form nanometer powder.
Described modified coal ash is prepared by following steps: first dried in 110 DEG C of baking ovens by flyash, then the flyash after oven dry is put into high-speed kneading machine, add be equivalent to flyash weight 5% aluminate coupling agent, 4% wooden sodium sulfonate, the triethyl citrate of 4%, the whiteruss of 2% and 5% talcum powder, after high-speed mixing, dry, pulverize and grind to form ultrafine powder.
The preparation method of the described environment-protective adhesive containing modified Nano bamboo charcoal powder, comprises following preparation process:
(1) by recipe ratio, just polyvinyl alcohol resin, 2-ethyl benzofuran, dibutyl phthalate, polystyrene, dixylenyl phosphate, isophorone diisocyanate, paracril, dibutyl tin laurate join reactor and are heated to 130 DEG C, high-speed stirring 3h;
(2) again other compositions are joined in the reactor in step (1), stir 2h, be cooled to normal temperature, pack.

Claims (3)

1. the environment-protective adhesive containing modified Nano bamboo charcoal powder, it is characterized in that: the component comprising following weight part: polyvinyl alcohol resin 100-150 part, 2-ethyl benzofuran 50-80 part, dibutyl phthalate 20-30 part, polystyrene 15-20 part, dixylenyl phosphate 10-15 part, isophorone diisocyanate 20-30 part, paracril 5-10 part, calcium carbonate 10-15 part, titanium dioxide 5-8 part, nano-sized magnesium hydroxide 5-20 part, modified Nano bamboo charcoal powder 15-20 part, xylogen 10-15 part, gas-phase silica 3-5 part, sodium alginate 3-5 part, quartz sand 20-30 part, boron powder 1-3 part, bath of glass 5-10 part, dibutyl tin laurate 0.7-0.9 part, iron mica 2-4 part, silane coupling agent 1-3 part, modified coal ash 10-15 part.
2. the environment-protective adhesive containing modified Nano bamboo charcoal powder according to claim 1, it is characterized in that: described modified coal ash is prepared by following steps: first flyash is dried in 100-110 DEG C of baking oven, then the flyash after oven dry is put into high-speed kneading machine, add be equivalent to flyash weight 3-5% aluminate coupling agent, the wooden sodium sulfonate of 2-4%, the triethyl citrate of 2-4%, the whiteruss of 1-2% and 2-5% talcum powder, after high-speed mixing, dry, pulverize and grind to form ultrafine powder.
3. the preparation method of the environment-protective adhesive containing modified Nano bamboo charcoal powder according to claim 1, is characterized in that: comprise following preparation process:
(1) by recipe ratio, just polyvinyl alcohol resin, 2-ethyl benzofuran, dibutyl phthalate, polystyrene, dixylenyl phosphate, isophorone diisocyanate, paracril, dibutyl tin laurate join reactor and are heated to 100-130 DEG C, high-speed stirring 3-4h;
(2) again other compositions are joined in the reactor in step (1), stir 1-2h, be cooled to normal temperature, pack.
CN201410057025.5A 2014-02-20 2014-02-20 Environment-friendly adhesive containing modified nanometer bamboo charcoal powder Expired - Fee Related CN103788911B (en)