[go: up one dir, main page]

CN103114445A - Shrink-proof finishing agent for wool fabrics and preparation method thereof - Google Patents

Shrink-proof finishing agent for wool fabrics and preparation method thereof Download PDF

Info

Publication number
CN103114445A
CN103114445A CN 201210442861 CN201210442861A CN103114445A CN 103114445 A CN103114445 A CN 103114445A CN 201210442861 CN201210442861 CN 201210442861 CN 201210442861 A CN201210442861 A CN 201210442861A CN 103114445 A CN103114445 A CN 103114445A
Authority
CN
China
Prior art keywords
parts
shrink
ethylene glycol
preparation
citric acid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN 201210442861
Other languages
Chinese (zh)
Inventor
钱树良
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
WUJIANG QIAN'S TEXTILE CO Ltd
Original Assignee
WUJIANG QIAN'S TEXTILE CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by WUJIANG QIAN'S TEXTILE CO Ltd filed Critical WUJIANG QIAN'S TEXTILE CO Ltd
Priority to CN 201210442861 priority Critical patent/CN103114445A/en
Publication of CN103114445A publication Critical patent/CN103114445A/en
Withdrawn legal-status Critical Current

Abstract

The invention discloses a shrink-proof finishing agent for wool fabrics and a preparation method thereof. The shrink-proof finishing agent for wool fabrics is prepared from the following components in parts by weight: 3-5 parts of citric acid, 3-6 parts of magnesium chloride, 1-3 parts of hydroxymethyl cellulose, 1-3 parts of sodium alginate, 2-5 parts of magnesium aluminum silicate, 10-30 parts of chitosan, 2-5 parts of sodium bicarbonate, 10-20 parts of ethylene glycol, 1-3 parts of dibutyl phthalate and 100-180 parts of water. Compared with the prior art, the shrink-proof finishing agent for wool fabrics does not need pretreatment, and has favorable compatibility with dye assistants for wool; and the preparation method has the advantages of simple technique and low cost.

Description

A kind of wool fabric shrink-resistant agent and preparation method thereof
Technical field
The invention belongs to the textile auxiliary technical field, more specifically relate to a kind of wool fabric shrink-resistant agent and preparation method thereof.
Background technology
Wool fibre has many premium properties, and its shortcoming is that wool fabric felting and fluffiness can occur when washing, and main cause is that wool surface has Microstructure of epidermal scale.Therefore, the shiinkproof finish of wool scale layer structure is the important research object of wool processing.The shiinkproof finish of wool fabric mainly contains two kinds of methods, and the one, adopt chemical treatments the phosphorus sheet of wool surface partly to be removed or removed fully, be called for short subtraction; Next is to adopt polymer treatment, and the scale on wool top layer is wrapped by, and mutually bonding between fiber, thereby gives its shrink resistance, is called for short addition.
Summary of the invention
The object of the invention is to overcome the deficiency that prior art exists, a kind of wool fabric shrink-resistant agent is provided.
Another object of the present invention is to provide the preparation method of this wool fabric shrink-resistant agent.
For achieving the above object, the present invention has taked following technical scheme:
A kind of wool fabric shrink-resistant agent in weight portion, consists of the following composition:
Citric acid: 3~5, magnesium chloride: 3~6, Carboxymethyl Cellulose: 1~3,
Sodium alginate: 1~3, Magnesiumaluminumsilicate: 2~5, chitin: 10~30,
Sodium bicarbonate: 2~5, ethylene glycol: 10~20, dibutyl phthalate: 1~3,
Water: 100~180.
In technique scheme, the preparation technology of described wool fabric shrink-resistant agent is as follows:
(1) dibutyl phthalate is added to the water, mixes;
(2) citric acid, chitin, ethylene glycol are mixed, stir;
(3) product with step (1) mixes with the product of step (2), stirring reaction 1~3 hour;
(4) add all the other components, get final product to get product after mixing.
Compared with prior art, the present invention has following beneficial effect:
(1) need not preliminary treatment, and good with the compatibility of color additive with hair;
(2) preparation technology is easy, and is with low cost.
The specific embodiment
The invention will be further described below in conjunction with specific embodiment, but the present invention's scope required for protection is not limited to the scope that embodiment describes.
Embodiment 1
A kind of wool fabric shrink-resistant agent in weight portion, consists of the following composition:
Citric acid: 3, magnesium chloride: 3, Carboxymethyl Cellulose: 1,
Sodium alginate: 1, Magnesiumaluminumsilicate: 2, chitin: 10,
Sodium bicarbonate: 2, ethylene glycol: 10, dibutyl phthalate: 1, water: 100.
Embodiment 2
A kind of wool fabric shrink-resistant agent in weight portion, consists of the following composition:
Citric acid: 5, magnesium chloride: 6, Carboxymethyl Cellulose: 3,
Sodium alginate: 3, Magnesiumaluminumsilicate: 5, chitin: 30,
Sodium bicarbonate: 5, ethylene glycol: 20, dibutyl phthalate: 3, water: 180.
Embodiment 3
A kind of wool fabric shrink-resistant agent in weight portion, consists of the following composition:
Citric acid: 4, magnesium chloride: 5, Carboxymethyl Cellulose: 2,
Sodium alginate: 2, Magnesiumaluminumsilicate: 4, chitin: 20,
Sodium bicarbonate: 3, ethylene glycol: 16, dibutyl phthalate: 2, water: 160.
In above-described embodiment, the preparation method of described a kind of wool fabric shrink-resistant agent comprises the steps:
(1) dibutyl phthalate is added to the water, mixes;
(2) citric acid, chitin, ethylene glycol are mixed, stir;
(3) product with step (1) mixes with the product of step (2), stirring reaction 1~3 hour;
(4) add all the other components, get final product to get product after mixing.

Claims (5)

1. a wool fabric shrink-resistant agent, is characterized in that, in weight portion, consists of the following composition:
Citric acid: 3~5, magnesium chloride: 3~6, Carboxymethyl Cellulose: 1~3,
Sodium alginate: 1~3, Magnesiumaluminumsilicate: 2~5, chitin: 10~30,
Sodium bicarbonate: 2~5, ethylene glycol: 10~20, dibutyl phthalate: 1~3,
Water: 100~180.
2. a kind of wool fabric shrink-resistant agent according to claim 1, is characterized in that, in weight portion, consists of the following composition:
Citric acid: 3, magnesium chloride: 3, Carboxymethyl Cellulose: 1,
Sodium alginate: 1, Magnesiumaluminumsilicate: 2, chitin: 10,
Sodium bicarbonate: 2, ethylene glycol: 10, dibutyl phthalate: 1, water: 100.
3. a kind of wool fabric shrink-resistant agent according to claim 1, is characterized in that, in weight portion, consists of the following composition:
Citric acid: 5, magnesium chloride: 6, Carboxymethyl Cellulose: 3,
Sodium alginate: 3, Magnesiumaluminumsilicate: 5, chitin: 30,
Sodium bicarbonate: 5, ethylene glycol: 20, dibutyl phthalate: 3, water: 180.
4. a kind of wool fabric shrink-resistant agent according to claim 1, is characterized in that, in weight portion, consists of the following composition:
Citric acid: 4, magnesium chloride: 5, Carboxymethyl Cellulose: 2,
Sodium alginate: 2, Magnesiumaluminumsilicate: 4, chitin: 20,
Sodium bicarbonate: 3, ethylene glycol: 16, dibutyl phthalate: 2, water: 160.
5. the preparation method of a kind of wool fabric shrink-resistant agent claimed in claim 1, is characterized in that, comprises the steps:
(1) dibutyl phthalate is added to the water, mixes;
(2) citric acid, chitin, ethylene glycol are mixed, stir;
(3) product with step (1) mixes with the product of step (2), stirring reaction 1~3 hour;
(4) add all the other components, get final product to get product after mixing.
CN 201210442861 2012-11-08 2012-11-08 Shrink-proof finishing agent for wool fabrics and preparation method thereof Withdrawn CN103114445A (en)