[go: up one dir, main page]

CN102508583B - 电容式触摸屏金属引线的制备方法 - Google Patents

电容式触摸屏金属引线的制备方法 Download PDF

Info

Publication number
CN102508583B
CN102508583B CN201110296985.3A CN201110296985A CN102508583B CN 102508583 B CN102508583 B CN 102508583B CN 201110296985 A CN201110296985 A CN 201110296985A CN 102508583 B CN102508583 B CN 102508583B
Authority
CN
China
Prior art keywords
glass substrate
ito
minute
deionized water
preparation
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201110296985.3A
Other languages
English (en)
Other versions
CN102508583A (zh
Inventor
丁建芳
张�雄
樊兆雯
朱立锋
林青园
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nanjing Panda Electronics Co Ltd
Original Assignee
Nanjing Panda Electronics Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nanjing Panda Electronics Co Ltd filed Critical Nanjing Panda Electronics Co Ltd
Priority to CN201110296985.3A priority Critical patent/CN102508583B/zh
Publication of CN102508583A publication Critical patent/CN102508583A/zh
Application granted granted Critical
Publication of CN102508583B publication Critical patent/CN102508583B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种电容式触摸屏金属引线的制备方法,其特征是首先通过丝网印刷树脂保护胶并热固化形成保护膜将双面带有ITO图形、四周有ITO引出线的玻璃基板上的ITO图形遮盖住,并将ITO引出线外露;其次,通过化学镀方法在玻璃基板四周的外露的ITO引出线表面依次覆盖铜和镍金属膜,形成触摸屏金属引线。用本发明方法制作的金属导线导电性能良好,与其他方法相制作工艺简单、成本较低。

Description

电容式触摸屏金属引线的制备方法
技术领域
本发明涉及一种电容式触摸屏制备技术,尤其是一种触摸屏上金属引线的制备方法,具体地说是一种通过化学镀铜和化学镀镍制作电容式触摸屏基板上金属引线的方法。
背景技术
为了降低电容式触摸屏周围引出线部分的电阻,触摸屏制作中将玻璃四周引出线制作成金属线条来获得良好的电性能。专利报道的金属引线制作方法有丝网印刷导电金属浆料制作金属线条【CN101996007A】溅射蒸镀金属膜后光刻并蚀刻制作金属线条【CN102096534A】,化学镀金方法制作金属引线【CN10184625A】。这些方法均存在制作工艺复杂、制作成本高的问题。
发明内容
本发明的目的是针对现有触摸屏金属引线制备工艺复杂,成本高的问题,发明一种成本低,工艺简单易行的电容式触摸屏金属引线的制备方法。
本发明的技术方案是:
一种电容式触摸屏金属引线的制备方法,其特征是首先通过丝网印刷树脂保护胶并热固化形成保护膜将双面带有ITO图形、四周有ITO引出线的玻璃基板上的ITO图形遮盖住,并将ITO引出线外露;其次,通过化学镀方法在玻璃基板四周的外露的ITO引出线表面依次覆盖铜和镍金属膜,最终形成触摸屏金属引线。
所述的化学镀铜和化学镀镍包括脱脂、粗化、胶体钯活化、解胶、化学镀铜、离子钯活化、化学镀镍和烘干:
(1)             脱脂:带有保护胶的玻璃基板浸入在40-50℃的中性脱脂液中3-5分钟,取出后用流动的去离子水冲洗玻璃;
(2)             粗化:玻璃基板放入pH值为1-3的酸性溶液中3-5分钟,用去离子水将玻璃基板冲洗干净;
(3)             胶体钯活化:玻璃基板浸入室温盐基钯胶体中3-5分钟,活化后在离子水中清洗玻璃基板;
(4)             解胶:玻璃基板浸入氢氧化钠溶液中10-60s,然后取出玻璃基板用去离子水冲洗干净;
(5)             化学镀铜:玻璃基板浸入温度在35-50℃pH值为11-12.5的化学镀铜液中1-3分钟,在玻璃基板四周的ITO引出线上形成1-5微米厚的铜膜覆盖,取出玻璃基板用去离子水冲洗干净;
(6)             离子钯活化:玻璃基板放入到离子钯活化液中1-2分钟,用去离子水将玻璃基板冲洗干净;
(7)             化学镀镍:玻璃基板放入80-95℃pH值为4-6的化学镀镍溶液中2-5分钟,在玻璃四周ITO引线的铜膜上形成3-6微米的镍金属层,用去离子水将玻璃基板冲洗干净;
(8)             去除玻璃基板图形区域ITO上覆盖的保护膜,将玻璃基板放入150℃烘箱,保温30分钟。
本发明的有益效果:
本发明采用化学镀铜和化学镀镍的方法在玻璃四周边缘形成铜镍金属引线,它具有制作工艺简化、制作成本低的优点。
具体实施方式
下面结合实施例对本发明作进一步的说明。
一种电容式触摸屏金属引线的制备方法,首先在玻璃基板上制作双面ITO图形,并在玻璃基板的四周形成ITO引出线,通过丝网印刷树脂保护胶遮盖住玻璃基板上的ITO图形,烘干后该保护胶和ITO图形以及玻璃基板之间具有良好的附着力,在强酸强碱的化学镀液中不发生化学、物理变化,不会脱落。
然后,将玻璃基板放入中性脱脂液中浸泡3~5分钟,脱脂液浓度为25g/L,温度为40~50℃,去除玻璃基板加工制作传递过程形成的油脂。脱脂后用流动的去离子水冲洗2分钟,将脱脂液完全冲洗干净。玻璃基板浸入室温下pH值为1~3,最佳为2的酸性溶液中3~5分钟,对玻璃基板上ITO引出线进行粗化,该粗化液由草酸、盐酸、硝酸、氢氟酸、氯化钠等组成,粗化后用去离子水将玻璃基板冲洗干净。玻璃基板浸入室温的胶体钯活化液中3~5分钟让钯胶团吸附在ITO表面,活化后用去离子水冲洗2分钟,该胶体钯中含有氯化钠、氯化钯、氯化亚锡,重量比分别为11%、0.02%、0.86%。玻璃基板浸入室温下、浓度为25g/L的氢氧化钠溶液中10-60秒最佳为15s,去离子水冲洗1分钟,目的是将胶团中的钯离子暴露出来。玻璃基板放入35~50℃,最佳为45℃、pH为11-12.5,最佳为12的化学镀铜液中1-3分钟,得到厚度为2微米的铜膜(也可将厚度控制在1-5微米以内),取出用去离子水冲洗干净。该化学镀铜液中硫酸铜16g/L、EDTA-2Na 25g/L、镀铜添加剂7mL/L、甲醛15mL/L、氢氧化钠14g/L。镀上铜膜的基板放入离子钯活化液中1-2分钟用去离子水冲洗干净,该离子钯中含有氯化钯0.1g/L、盐酸0.2g/L。将玻璃基板放入85℃(也可为80-95℃)pH值为4.5(也可为4-6)的镀镍溶液中2-5分钟在铜膜上得到厚度为3微米(也可介于3-6微米之间)的镍膜,在离子水下冲洗干净。化学镀镍液中化学组成有硫酸镍25g/L、乳酸25mL/L、醋酸钠15g/L、次亚磷酸钠30g/L、化学镍添加剂5mL/L。通过化学镀方法形成铜和镍金属导线触摸屏基板,去除基板上ITO图形区域的保护膜,放入150℃干燥箱里保温30分钟使金属膜和基板之间的附着力进一步坚固。
本发明未涉及部分均与现有技术相同或可采用现有技术加以实现。

Claims (1)

1.一种电容式触摸屏金属引线的制备方法,其特征是首先通过丝网印刷树脂保护胶并热固化形成保护膜将双面带有ITO图形、四周有ITO引出线的玻璃基板上的ITO图形遮盖住,并将ITO引出线外露;其次,通过化学镀方法在玻璃基板四周外露的ITO引出线表面依次覆盖铜和镍金属膜,形成触摸屏金属引线;所述的化学镀铜和化学镀镍包括脱脂、粗化、胶体钯活化、解胶、化学镀铜、离子钯活化、化学镀镍和烘干:
脱脂:带有保护胶的玻璃基板浸入在40-50℃的中性脱脂液中3-5分钟,取出后用流动的去离子水冲洗玻璃;
粗化:玻璃基板放入pH值为1-3的酸性溶液中3-5分钟,用去离子水将玻璃基板冲洗干净;
胶体钯活化:玻璃基板浸入室温盐基钯胶体中3-5分钟,活化后在离子水中清洗玻璃基板;
解胶:玻璃基板浸入氢氧化钠溶液中10-60s,然后取出玻璃基板用去离子水冲洗干净;
化学镀铜:玻璃基板浸入温度为35-50℃pH值为11-12.5的化学镀铜液中1-3分钟,在玻璃基板四周的ITO引出线上形成1-5微米厚的铜膜覆盖,取出玻璃基板用去离子水冲洗干净;
离子钯活化:玻璃基板放入到离子钯活化液中1-2分钟,用去离子水将玻璃基板冲洗干净;
化学镀镍:玻璃基板放入80-95℃pH值为4-6的化学镀镍溶液中2-5分钟,在玻璃四周ITO引线的铜膜上形成3-6微米的镍金属层,用去离子水将玻璃基板冲洗干净;
烘干:去除玻璃基板图形区域ITO上覆盖的树脂保护膜,将玻璃基板放入150℃烘箱,保温30分钟。
CN201110296985.3A 2011-09-30 2011-09-30 电容式触摸屏金属引线的制备方法 Expired - Fee Related CN102508583B (zh)