JP6782676B2 - Polarizing plate and liquid crystal display device - Google Patents
Polarizing plate and liquid crystal display device Download PDFInfo
- Publication number
- JP6782676B2 JP6782676B2 JP2017193521A JP2017193521A JP6782676B2 JP 6782676 B2 JP6782676 B2 JP 6782676B2 JP 2017193521 A JP2017193521 A JP 2017193521A JP 2017193521 A JP2017193521 A JP 2017193521A JP 6782676 B2 JP6782676 B2 JP 6782676B2
- Authority
- JP
- Japan
- Prior art keywords
- film
- polarizing
- polarizing plate
- protective film
- liquid crystal
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Description
本発明は、偏光板及び液晶表示装置に関する。 The present invention relates to a polarizing plate and a liquid crystal display device.
近年、液晶ディスプレイ用の液晶パネルは薄肉化が求められている。液晶パネルに用いられる偏光子は一般に脆くて裂けやすいため、これを保護するべく偏光子の両面に保護フィルムを貼合して偏光板を構成し(例えば、特許文献1参照)、これを液晶セルに貼着する。 In recent years, liquid crystal panels for liquid crystal displays have been required to be thinner. Polarizers used in liquid crystal panels are generally brittle and easily torn, so in order to protect them, protective films are attached to both sides of the polarizer to form a polarizing plate (see, for example, Patent Document 1), which is used as a liquid crystal cell. Attach to.
液晶パネルの更なる薄肉化要求により、偏光子の片面にのみ保護フィルムを貼合した偏光板の開発が行われている。しかしながら、偏光子の片面にのみ保護フィルムを貼合した偏光板は、耐久試験時に偏光子にクラックが入りやすい傾向がある。 Due to the demand for further thinning of the liquid crystal panel, a polarizing plate in which a protective film is attached to only one side of the polarizer is being developed. However, a polarizing plate in which a protective film is attached to only one side of the polarizing element tends to have cracks in the polarizing element during a durability test.
そこで本発明は、偏光子の片面のみに保護フィルムを備える偏光板であって、耐久試験時にクラックが入りにくい偏光板を提供することを目的とする。また、当該偏光板を備える液晶表示装置を提供することを目的とする。 Therefore, an object of the present invention is to provide a polarizing plate having a protective film on only one side of the polarizer, which is less likely to crack during a durability test. Another object of the present invention is to provide a liquid crystal display device provided with the polarizing plate.
本発明は、偏光子と、その片面のみに接着剤を介して積層された保護フィルムと、を備える偏光板であって、保護フィルムは、所定の形状に成形されたものであり、保護フィルムは、偏光子の片面の全面に積層されており、偏光子の少なくとも一部の端部が、保護フィルムの端部よりも内側に位置している偏光板を提供する。 The present invention is a polarizing plate including a polarizing element and a protective film laminated on only one side thereof via an adhesive. The protective film is formed into a predetermined shape, and the protective film is Provided is a polarizing plate which is laminated on the entire surface of one side of a polarizing element, and at least a part of the ends of the polarizer is located inside the end of the protective film.
この偏光板では、偏光子の端部が保護フィルムの端部よりも内側に位置しているため、偏光子の端部が物理的に保護される。従って、偏光板のハンドリングにおいて偏光板の側面が衝撃を受けた場合に、偏光子の端部に傷やクラックが生じることが防止される。また、耐久試験時にもクラックが入りにくい。 In this polarizing plate, since the end of the polarizer is located inside the end of the protective film, the end of the polarizer is physically protected. Therefore, when the side surface of the polarizing plate is impacted in the handling of the polarizing plate, it is possible to prevent scratches and cracks from being generated at the end of the polarizer. In addition, cracks are unlikely to occur during the durability test.
この偏光板において、偏光子の全ての端部が保護フィルムの端部よりも内側に位置していてもよい。この場合、偏光子の全ての端部が保護される。 In this polarizing plate, all the ends of the polarizer may be located inside the edges of the protective film. In this case, all ends of the polarizer are protected.
この偏光板は、偏光子における保護フィルムが積層されている側とは反対側の面、及び、保護フィルムにおける偏光子が積層されている側とは反対側の面の少なくとも一方の面に積層された粘着剤層を更に備えていてもよく、この粘着剤層を介して積層された光学機能フィルムを更に備えていてもよい。光学機能フィルムとしては、反射型偏光子が挙げられる。 This polarizing plate is laminated on at least one surface of the protector opposite to the side on which the protective film is laminated and the surface of the protective film opposite to the side on which the protector is laminated. The pressure-sensitive adhesive layer may be further provided, and an optical functional film laminated via the pressure-sensitive adhesive layer may be further provided. Examples of the optical functional film include a reflective polarizer.
また、本発明は、上記偏光板を備える液晶表示装置を提供する。上記偏光板を液晶セル等に貼着させた液晶表示装置を構成した場合でも、偏光子の端部が物理的に保護される。 The present invention also provides a liquid crystal display device including the above-mentioned polarizing plate. Even when a liquid crystal display device in which the above-mentioned polarizing plate is attached to a liquid crystal cell or the like is configured, the end portion of the polarizer is physically protected.
本発明によれば、偏光子の片面のみに保護フィルムを備える偏光板であって、耐久試験時にクラックが入りにくい偏光板を提供することができる。また、当該偏光板を備える液晶表示装置を提供することができる。 According to the present invention, it is possible to provide a polarizing plate having a protective film on only one side of the polarizer, which is less likely to crack during a durability test. Further, it is possible to provide a liquid crystal display device provided with the polarizing plate.
以下、本発明の好適な実施形態について、図面を参照しながら詳細に説明する。なお、各図において同一部分又は相当部分には同一符号を付し、重複する説明は省略する。また、各図面の寸法比率は必ずしも実際のものとは一致せず、特に、フィルムの厚さに関しては誇張して描いてある。 Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings. In each figure, the same parts or corresponding parts are designated by the same reference numerals, and duplicate description will be omitted. In addition, the dimensional ratio of each drawing does not always match the actual one, and in particular, the thickness of the film is exaggerated.
<第1の実施形態>
図1及び図2に示されているとおり、本実施形態の偏光板1Aは、薄膜状に形成された偏光フィルム(偏光子)2の片面に、接着剤層4を介して保護フィルム3が積層されて成っている。偏光フィルム2及び保護フィルム3は平面視長方形に成形されており、この形状が偏光板1Aの外観形状ともなっている。
<First Embodiment>
As shown in FIGS. 1 and 2, in the polarizing
偏光板1Aは、液晶セル等の表示用セル(画像表示素子)の片面又は両面に貼合されるものである。偏光板1は、表示用セルの背面側に貼合されることが好ましい。背面側の偏光板は視認側の偏光板に比べて結露等が生じやすく偏光フィルムにクラックが入りやすいところ、本実施形態の偏光板1によれば偏光フィルム2にクラックが入ることを顕著に抑制することができる。
The polarizing
偏光フィルム2の端部2aは、その全周に亘って、保護フィルム3の端部3aよりも内側(偏光板1の主面の中央側)に凹んで位置している。すなわち、図2に示された断面図において、偏光板1Aの側面は、偏光フィルム2の側面が保護フィルム3の側面に対して凹んだ形状をなしている。
The
ここで「偏光フィルム2の端部2a」とは、偏光フィルム2の端面を構成する辺のうち保護フィルム3から遠い側にあって偏光板1の厚さ方向に垂直な辺をいう。また、「保護フィルム3の端部3a」とは、保護フィルム3の端面を構成する辺のうち偏光フィルム2から遠い側にあって偏光板1の厚さ方向に垂直な辺をいう。
Here, the "
偏光フィルム2の端部2aは、保護フィルム3の端部3aよりも1〜500μm内側に位置していることが好ましく、2〜300μm内側に位置していることがより好ましく、5〜50μm内側に位置していることが更に好ましい。なかでも、本実施形態のように、偏光フィルム2の全周に亘って同じ長さで内側に位置していることが好ましい。偏光フィルム2の端部2aがこれらの範囲に位置していると、偏光フィルム2の端部2aを物理的に保護する効果が特に高く、液晶表示装置を構成した場合にも表示面を広く確保することができる。
The
偏光フィルム2と保護フィルム3とは、接着剤層4を介して貼合して積層されている。
The polarizing
偏光フィルム2の材料としては、従来から偏光板の製造に使用されている公知の材料を用いることができ、例えば、ポリビニルアルコール系樹脂、ポリ酢酸ビニル樹脂、エチレン/酢酸ビニル(EVA)樹脂、ポリアミド樹脂、ポリエステル系樹脂等が挙げられる。なかでもポリビニルアルコール系樹脂が好ましい。保護フィルム3と貼合するためにフィルム状に成形する場合は、一軸延伸したフィルムにヨウ素又は二色性染料による染色を施し、ついでホウ酸処理することが好ましい。後述するとおり、フィルム状の偏光子は、偏光板の製造時に任意の大きさに切り出して用いることができる。
As the material of the polarizing
偏光フィルム2の厚さは、2〜30μmであることが好ましく、2〜15μmであることがより好ましく、2〜10μmであることが更に好ましい。一般に偏光フィルムは薄いほどクラックが入りやすいが、本実施形態では偏光フィルム2が10μm以下であっても顕著にクラックを防止し得る。
The thickness of the polarizing
保護フィルム3は、偏光フィルム2の主面や端部の割れや傷つきを防止するフィルムである。ここで「保護フィルム」とは、偏光フィルム2に種々積層され得るフィルムのなかでも、偏光フィルム2に最も近い位置に物理的に積層されたフィルムを指している。
The
保護フィルム3は、偏光板の分野で知られている各種の透明樹脂フィルムで構成することができる。例えば、トリアセチルセルロースを代表例とするセルロース系樹脂、ポリプロピレン系樹脂を代表例とするポリオレフィン系樹脂、ノルボルネン系樹脂を代表例とする環状オレフィン系樹脂、ポリメチルメタクリレート系樹脂を代表例とするアクリル系樹脂、ポリエチレンテレフタレート系樹脂を代表例とするポリエステル系樹脂等が挙げられる。なかでも、セルロース系樹脂が代表的である。
The
保護フィルム3の厚さは、5〜90μmであることが好ましく、5〜80μmであることがより好ましく、5〜50μmであることが更に好ましい。
The thickness of the
接着剤層4を構成する接着剤としては、従来から偏光板の製造に使用されている各種の接着剤を使用することができる。例えば、耐候性や屈折率、カチオン重合性等の観点から、分子内に芳香環を含まないエポキシ樹脂が好ましい。また、活性エネルギー線(紫外線又は熱線)の照射によって硬化するものが好ましく、カチオン系紫外線硬化性接着剤、ラジカル系紫外線硬化性接着剤が特に好ましい。
As the adhesive constituting the
エポキシ樹脂としては、例えば水素化エポキシ樹脂、脂環式エポキシ樹脂、脂肪族エポキシ樹脂等が好ましい。エポキシ樹脂に対して、重合開始剤(例えば紫外線照射で重合させるための光カチオン重合開始剤、熱線照射によって重合させるための熱カチオン重合開始剤)や、更に他の添加剤(増感剤等)を添加して、塗布用のエポキシ樹脂組成物を調製して使用することができる。 As the epoxy resin, for example, a hydrogenated epoxy resin, an alicyclic epoxy resin, an aliphatic epoxy resin and the like are preferable. Polymerization initiators (for example, photocationic polymerization initiators for polymerizing by ultraviolet irradiation, thermal cationic polymerization initiators for polymerizing by heat ray irradiation) and other additives (sensitizers, etc.) for epoxy resins. Can be added to prepare and use an epoxy resin composition for coating.
ラジカル系紫外線硬化性接着剤を構成する樹脂としては、分子中に1個以上の(メタ)アクリロイルオキシ基を有する(メタ)アクリル系化合物を含有し、重合開始剤の存在下において活性エネルギー線(たとえば、紫外線、可視光、電子線、X線など)の照射により重合可能な(メタ)アクリル系化合物が挙げられる。 The resin constituting the radical ultraviolet curable adhesive contains a (meth) acrylic compound having one or more (meth) acryloyloxy groups in the molecule, and is an active energy ray (active energy ray) in the presence of a polymerization initiator. For example, (meth) acrylic compounds that can be polymerized by irradiation with ultraviolet rays, visible light, electron beams, X-rays, etc. can be mentioned.
また、接着剤としては、アクリルアミド、アクリレート、ウレタンアクリレート、エポキシアクリレート等のアクリル系樹脂を含む組成物や、ポリビニルアルコール系樹脂を含む水系接着剤を使用することもできる。 Further, as the adhesive, a composition containing an acrylic resin such as acrylamide, acrylate, urethane acrylate, or epoxy acrylate, or a water-based adhesive containing a polyvinyl alcohol-based resin can also be used.
偏光フィルム2、接着剤層4、及び保護フィルム3の三層からなる偏光板1Aの厚さは、7〜120μmであることが好ましく、10〜70μmであることがより好ましく、10〜55μmであることが更に好ましい。
The thickness of the
偏光板1Aは、例えば以下のようにして製造することができる。まず、保護フィルム3を構成する材料からなる長尺のフィルムロールから、保護フィルム3を長方形に切り出す。切り出す長方形の大きさや縦横比は、偏光板1Aの適用対象に応じて決めたものとする。保護フィルム3の片面に接着剤を塗布する。接着剤を塗布する領域は保護フィルム3の全面ではなく、偏光フィルム2が積層される領域とする。
The
次に、偏光フィルム2を構成する材料からなる長尺のフィルムロールから、偏光フィルム2を長方形に切り出す。切り出す長方形の大きさは、保護フィルム3の大きさよりも小さくする。小さくする分量としては、偏光フィルム2の端部2aを保護フィルム3の端部3aよりも内側に凹ませたい分とする。切り出したフィルム状の偏光フィルム2を、接着剤を塗布した保護フィルム3の面に、例えば貼合ロールを用いて積層する。ここでの積層は、偏光フィルム2の片面の全面が保護フィルム3の面の内側に入るように行う。ここで保護フィルム3側から見れば、偏光フィルム2は保護フィルム3に覆われている。接着剤として活性エネルギー線硬化性樹脂を用いた場合は、ここで活性エネルギー線を照射して接着剤を硬化させる。
Next, the
以上の手順によって、偏光板1Aが製造される。
The
以上に説明した偏光板1Aは、偏光フィルム2の端部2aが保護フィルム3の端部3aよりも内側に位置しているため、偏光フィルム2の端部2aが物理的に保護される。従って、偏光板1Aを例えば液晶セルに貼り付ける場合のようなハンドリングにおいて、偏光板1Aの側面が衝撃を受けた場合に、保護フィルム3の端部3aのみが衝撃を受けることとなり、偏光フィルム2の端部に傷やクラックが生じることが防止される。この効果は、偏光板1Aを液晶セル等に貼り付けた後の更なるハンドリングにおいても奏される。また、偏光板1Aはヒートショック試験等の耐久試験において偏光フィルム2にクラックが入りにくい。
In the
また、偏光板1Aは、保護フィルム3の端部3aによって偏光フィルム2の端部2aが保護されているため、特に近年の液晶セルの狭額縁化傾向において、その効果が良好に奏される。すなわち、偏光板1Aが貼着された液晶セルの額縁が通常幅である場合は、偏光フィルム2に物理的衝撃が加わることを液晶セル自体が保護する働きがあるが、液晶セルが狭額縁であると、その保護の効果が小さくなる。この場合、液晶セル側の保護フィルム3の端部3aが偏光フィルム2の端部2aの保護に寄与する割合が大きくなる。
Further, since the
偏光フィルム2の端部2aは全周に亘って保護フィルム3の端部3aよりも内側にあるため、上記の効果は、偏光板1Aの全周に亘って奏される。
Since the
また、偏光板1Aは平面視長方形であるため、液晶表示装置等、種々の物品に適用しやすい。
Further, since the
<第2の実施形態>
偏光板1Aは、他の光学機能フィルムを更に備えていてもよい。他の光学機能フィルムとしては、ある種の偏光を透過し、それと逆の性質を示す偏光を反射する反射型偏光子;表面に凹凸形状を有する防眩機能付フィルム;表面反射防止機能付フィルム;表面に反射機能を有する反射フィルム;反射機能と透過機能とを併せ持つ半透過反射フィルム;視野角補償フィルム;位相差フィルム等が挙げられる。以下では反射型偏光子を備える態様について説明する。
<Second embodiment>
The
図3に示されているとおり、偏光板1Bは、偏光フィルム2、接着剤層4及び保護フィルム3からなる偏光板の偏光フィルム2側の面に、粘着剤層5を介して反射型偏光子6が積層されている。
As shown in FIG. 3, the
反射型偏光子6の大きさ及び形状は、保護フィルム3の大きさ及び形状と同一とされており、その端部は偏光フィルム2の端部から張り出している。反射型偏光子6としては、任意のものを用いることができる。
The size and shape of the reflective
粘着剤層5は、アクリル系樹脂や、シリコーン系樹脂、ポリエステル、ポリウレタン、ポリエーテル等で構成することができる。
The pressure-
粘着剤層5の厚さは、2〜50μmであることが好ましく、2〜40μmであることがより好ましく、2〜30μmであることが更に好ましい。
The thickness of the pressure-
粘着剤層5を偏光フィルム2に積層する方法としては、例えば、偏光フィルム2に上記樹脂や任意の添加成分を含む溶液を塗布する方法でもよく、別途用意したセパレータ上に当該溶液で粘着剤層5を形成した後にこれを偏光フィルム2に転写する方法でもよい。
As a method of laminating the pressure-
偏光板1Bは、他の物品に貼着する目的のために、反射型偏光子6上に更に別の粘着剤層(図示せず)を備え、これにセパレータ(図示せず)が積層されていてもよい。
The
セパレータは、粘着剤層の保護や異物の付着防止等を目的として貼着される剥離可能なフィルムであって、偏光板1Bの使用時に剥がされて粘着剤層が露出される。セパレータは、例えばポリエチレンのようなポリエチレン系樹脂、ポリプロピレンのようなポリプロピレン系樹脂、ポリエチレンテレフタレートのようなポリエステル系樹脂等で構成することができる。中でも、ポリエチレンテレフタレートの延伸フィルムが好ましい。
The separator is a peelable film that is attached for the purpose of protecting the pressure-sensitive adhesive layer, preventing foreign matter from adhering, and the like, and is peeled off when the
偏光板1Bによれば、偏光フィルム2が損傷、摩損することが防止される。また、反射型偏光子6の端部が偏光フィルム2の端部2aよりも張り出していることによって、偏光フィルム2の端部2aが一層保護されている。
According to the
なお、反射型偏光子6の大きさ及び形状は、図4に示されている偏光板1Cのように、偏光フィルム2の大きさ及び形状と同一としてもよい。
The size and shape of the
また、保護フィルム3上に更に粘着剤層5を備えている場合は、図5に示されているとおり、例えば偏光板1Bを液晶セル8の背面側(図示下側)に貼着し、他方、偏光フィルム2側の表面に粘着剤層5を備えた偏光板1Aを液晶セル8の視認側(図示上側)に貼着して液晶パネル9を構成し、これにバックライト(面光源装置;図示省略)その他の部材を組み合わせることで、液晶表示装置10を作製することができる。なお、液晶表示装置には、通常2枚の偏光板が組み込まれるが、本実施形態の液晶表示装置としては、偏光板を少なくとも1枚備えていればよい。
When the
以上、本発明の好適な実施形態について説明したが、本発明は上記実施形態に何ら限定されるものではない。例えば、上記実施形態では偏光フィルム2の端部2aがその全周に亘って保護フィルム3の端部3aよりも内側に位置している態様を示したが、内側に位置する部分が偏光フィルム2の全周に亘っていなくてもよい。この場合、偏光フィルム2の端部2aは、保護フィルム3の端部3aよりも内側に位置している部分のみが保護される。
Although the preferred embodiment of the present invention has been described above, the present invention is not limited to the above embodiment. For example, in the above embodiment, the
また、上記実施形態では偏光フィルム2の全周に亘って同じ長さで内側に位置している様子を示したが、場所によって偏光フィルム2の凹みの程度を変えてもよい。例えば、偏光板のハンドリング時に衝撃を受けやすい部分があらかじめ分かっている場合は、その部分の偏光フィルムの端部の凹み幅を大きくしておくことが好ましい。
Further, in the above embodiment, it is shown that the
また、上記実施形態では偏光板1A,1Bが平面視長方形である例を示したが、他の四角形、例えば台形、平行四辺形、正方形等であってもよいほか、円形や楕円形であってもよい。すなわち偏光板1A,1Bは、偏光板1A,1Bを貼着する物品の形状に合わせて任意の形状とすることができる。
Further, in the above embodiment, an example in which the
また、第2の実施形態では粘着剤層5が偏光フィルム2側に積層された態様を示したが、保護フィルム3側にも粘着剤層5が積層し、他の光学機能層を積層した態様としてもよい。
Further, in the second embodiment, the
以下、実施例及び比較例を挙げて本発明の内容をより具体的に説明する。なお、本発明は下記実施例に限定されるものではない。 Hereinafter, the contents of the present invention will be described more specifically with reference to Examples and Comparative Examples. The present invention is not limited to the following examples.
(1)偏光フィルムの作製
平均重合度約2400、ケン化度99.9モル%以上で厚み20μmのポリビニルアルコールフィルムを、乾式で約4倍に一軸延伸した。延伸の緊張状態を保ったまま、40℃の純水に1分間浸漬した後、ヨウ素/ヨウ化カリウム/水の重量比が0.1/5/100である水溶液に28℃で60秒間浸漬した。その後、ヨウ化カリウム/ホウ酸/水の重量比が10.5/7.5/100である水溶液に68℃で300秒間浸漬した。引き続き、5℃の純水で5秒間洗浄した後、70℃で180秒間乾燥して、一軸延伸されたポリビニルアルコールフィルムにヨウ素が吸着配向された偏光フィルム(偏光子)を得た。偏光フィルムの厚さは7μmであった。
(1) Preparation of Polarizing Film A polyvinyl alcohol film having an average degree of polymerization of about 2400, a saponification degree of 99.9 mol% or more and a thickness of 20 μm was uniaxially stretched about 4 times by a dry method. After immersing in pure water at 40 ° C. for 1 minute while maintaining the tension of stretching, it was immersed in an aqueous solution having a weight ratio of iodine / potassium iodide / water of 0.1 / 5/100 at 28 ° C. for 60 seconds. .. Then, it was immersed in an aqueous solution having a weight ratio of potassium iodide / boric acid / water of 10.5 / 7.5 / 100 at 68 ° C. for 300 seconds. Subsequently, the film was washed with pure water at 5 ° C. for 5 seconds and then dried at 70 ° C. for 180 seconds to obtain a polarizing film (polarizer) in which iodine was adsorbed and oriented on a uniaxially stretched polyvinyl alcohol film. The thickness of the polarizing film was 7 μm.
(2)接着剤の調製
(2−1)水系接着剤
ポリビニルアルコール粉末(株式会社クラレ製の商品名「KL−318」、平均重合度1800)を95℃の熱水に溶解し、濃度3重量%のポリビニルアルコール水溶液を調製した。得られた水溶液に架橋剤(田岡化学工業株式会社製の商品名「スミレーズレジン650」〕をポリビニルアルコール粉末2質量部に対して1質量部の割合で混合して、水系接着剤とした。
(2) Preparation of Adhesive (2-1) Water-based Adhesive Polyvinyl alcohol powder (trade name "KL-318" manufactured by Kuraray Co., Ltd., average degree of polymerization of 1800) is dissolved in hot water at 95 ° C. to a concentration of 3 weight. % Polyvinyl alcohol aqueous solution was prepared. A cross-linking agent (trade name "Smiley's Resin 650" manufactured by Taoka Chemical Industry Co., Ltd.) was mixed with the obtained aqueous solution at a ratio of 1 part by mass with respect to 2 parts by mass of polyvinyl alcohol powder to obtain an aqueous adhesive.
(2−2)カチオン系紫外線硬化性接着剤
以下の各成分を混合し、脱泡して紫外線硬化性接着剤を調製した。なお、光カチオン重合開始剤は、50%プロピレンカーボネート溶液の形で入手したものを使用した。以下に示す配合量(2.25質量部)は、固形分量である。
・3,4−エポキシシクロヘキシルメチル 3,4−エポキシシクロヘキサンカルボキシレート … 75質量部
・1,4−ブタンジオールジグリシジルエーテル … 20質量部
・2−エチルヘキシルグリシジルエーテル … 5質量部
・トリアリールスルホニウム ヘキサフルオロホスフェート系の光カチオン重合開始剤 … 2.25質量部
(2-2) Cationic UV Curable Adhesive The following components were mixed and defoamed to prepare an UV curable adhesive. As the photocationic polymerization initiator, one obtained in the form of a 50% propylene carbonate solution was used. The blending amount (2.25 parts by mass) shown below is the amount of solid content.
・ 3,4-
(2−3)ラジカル系紫外線硬化性接着剤
以下の各成分を混合し、脱泡して紫外線硬化性接着剤を調製した。
・ビス(3−エチル−3−オキセタニルメチル)エーテル(アロンオキセタン OXT−221、東亞合成株式会社製) … 15質量部
・トリシクロデカンジメタノールジアクリレート(A−DCP、新中村化学工業株式会社製) … 50質量部
・2−ヒドロキシ−2−メチル−1−フェニルプロパン−1−オン(DAROCUR 1173、チバ・スペシャルティ・ケミカルズ社製)(光ラジカル重合開始剤) … 2.25質量部
(2-3) Radical-based UV-curable adhesive The following components were mixed and defoamed to prepare an UV-curable adhesive.
・ Bis (3-ethyl-3-oxetanylmethyl) ether (Aron oxetane OXT-221, manufactured by Toa Synthetic Co., Ltd.)… 15 parts by mass ・ Tricyclodecanedimethanol diacrylate (A-DCP, manufactured by Shin-Nakamura Chemical Industry Co., Ltd.) )… 50 parts by mass ・ 2-Hydroxy-2-methyl-1-phenylpropan-1-one (DAROCUR 1173, manufactured by Ciba Specialty Chemicals) (photoradical polymerization initiator)… 2.25 parts by mass
(3)片面保護偏光板の作製(水系接着剤を用いる場合)
次の手順で剥離フィルム付片面保護偏光板を作製した。上記(1)で得られた偏光フィルムと、保護フィルム(日本ゼオン株式会社製 ゼオノアフィルム ゼオノアフィルムZF14−023、厚さ23μm)のロールから保護フィルムを1枚ずつ120mm×70mmのサイズで切り出した。このとき、偏光フィルムが保護フィルムよりもわずかに小さくなるように調整した(「わずかに」の程度については後述する)。保護フィルムにはコロナ処理を施し、また、剥離フィルム(コニカミノルタオプト(株)製のTACフィルムである商品名「KC8UX2MW」、厚み80μm、ケン化処理なし)を別途切り出して、保護フィルム、偏光フィルム、剥離フィルムの順に積層した。
(3) Fabrication of single-sided protective polarizing plate (when using water-based adhesive)
A single-sided protective polarizing plate with a release film was produced by the following procedure. A protective film having a size of 120 mm × 70 mm was cut out from a roll of the polarizing film obtained in (1) above and a protective film (Zeonor film Zeonoa film ZF14-023, thickness 23 μm) manufactured by Nippon Zeon Corporation. At this time, the polarizing film was adjusted to be slightly smaller than the protective film (the degree of "slightly" will be described later). The protective film is corona-treated, and a release film (trade name "KC8UX2MW", which is a TAC film manufactured by Konica Minolta Opto Co., Ltd., thickness 80 μm, no saponification treatment) is separately cut out to form a protective film and a polarizing film. , The release film was laminated in this order.
次いで、偏光フィルムと保護フィルムとの間に上記(2−1)で得られた水系接着剤を注入するとともに、偏光フィルムと剥離フィルムとの間に純水を注入し、貼合ロール間に通して保護フィルム/水系接着剤層/偏光フィルム/純水/剥離フィルムからなる積層フィルムとした。引き続き、積層フィルムを、乾燥装置内で80℃、300秒の加熱処理を行うことにより、水系接着剤層を乾燥するとともに、偏光フィルムと剥離フィルムの間に介在する純水を揮発除去して、剥離フィルム付片面保護偏光板を得た。剥離フィルム付片面保護偏光板から剥離フィルムを剥離し、片面保護偏光板を得た。 Next, the water-based adhesive obtained in (2-1) above is injected between the polarizing film and the protective film, and pure water is injected between the polarizing film and the release film and passed between the bonding rolls. A laminated film composed of a protective film, a water-based adhesive layer, a polarizing film, pure water, and a release film. Subsequently, the laminated film was heat-treated at 80 ° C. for 300 seconds in a drying device to dry the aqueous adhesive layer and volatilize and remove the pure water interposed between the polarizing film and the release film. A single-sided protective polarizing plate with a release film was obtained. The release film was peeled off from the single-sided protective polarizing plate with a release film to obtain a single-sided protective polarizing plate.
(4)片面保護偏光板の作製(紫外線硬化性接着剤を用いる場合)
上記(1)で得られた偏光フィルムと、保護フィルム(日本ゼオン株式会社製 ゼオノアフィルム ゼオノアフィルムZF14−023、厚さ23μm)のロールから保護フィルムを1枚ずつ切り出した。このとき、偏光フィルムが保護フィルムよりも小さくなるように調整した。保護フィルムにはコロナ処理を施し、保護フィルム、偏光フィルムの順に積層した。
(4) Fabrication of single-sided protective polarizing plate (when using UV-curable adhesive)
A protective film was cut out one by one from a roll of the polarizing film obtained in (1) above and a protective film (Zeon Corporation Zeonoa Film Zeonoa Film ZF14-023, thickness 23 μm). At this time, the polarizing film was adjusted to be smaller than the protective film. The protective film was subjected to corona treatment, and the protective film and the polarizing film were laminated in this order.
次いで、偏光フィルムと保護フィルムとの間に上記(2−2)又は(2−3)で得られた紫外線硬化性接着剤を注入し、貼合ロール間に通して保護フィルム/紫外線硬化性接着剤/偏光フィルムからなる積層フィルムとした。引き続き、UV照射装置を用いて、保護フィルム側からUV照射を行うことにより、紫外線硬化性接着剤を硬化させて、片面保護偏光板を得た。 Next, the ultraviolet curable adhesive obtained in (2-2) or (2-3) above is injected between the polarizing film and the protective film, and the protective film / ultraviolet curable adhesive is passed between the bonding rolls. A laminated film composed of an agent / polarizing film was used. Subsequently, UV irradiation was performed from the protective film side using a UV irradiation device to cure the ultraviolet curable adhesive to obtain a single-sided protective polarizing plate.
(5)輝度向上フィルム付片面保護偏光板の作製
上記(3)及び(4)で得られた片面保護偏光板の偏光フィルム面にアクリル系感圧式粘着剤を介して、輝度向上フィルム(3M株式会社製の反射型偏光子である商品名「APF」)を貼合して輝度向上フィルム付片面保護偏光板を得た。このとき、輝度向上フィルムのサイズは偏光板のサイズと同じとし、偏光フィルムの延伸方向に対して、輝度向上フィルムの延伸軸を平行にして貼合した。
(5) Preparation of Single-sided Protective Polarizing Plate with Brightness-Improved Film Brightness-improving film (3M stock) on the polarizing film surface of the single-sided protective polarizing plate obtained in (3) and (4) above with an acrylic pressure-sensitive adhesive. A single-sided protective polarizing plate with a brightness-improving film was obtained by laminating (trade name "APF"), which is a reflective polarizer manufactured by the company. At this time, the size of the brightness improving film was the same as the size of the polarizing plate, and the stretching axis of the brightness improving film was parallel to the stretching direction of the polarizing film and bonded.
(6)アクリル系感圧式粘着剤付偏光板の作製
上記(5)で得られた輝度向上フィルム付片面保護偏光板の輝度向上フィルム面にセパレータフィルム付きアクリル系感圧式粘着剤を貼合してアクリル系感圧式粘着剤付偏光板を得た。
(6) Preparation of Polarizing Plate with Acrylic Pressure-Sensitive Adhesive Acrylic pressure-sensitive adhesive with separator film is attached to the brightness-enhancing film surface of the single-sided protective polarizing plate with brightness-enhancing film obtained in (5) above. A polarizing plate with an acrylic pressure-sensitive adhesive was obtained.
(7)ヒートショック試験
耐久試験として、ヒートショック試験を行った。ヒートショック試験用のサンプルは以下の手順で作製した。
(7) Heat shock test A heat shock test was conducted as a durability test. A sample for the heat shock test was prepared by the following procedure.
上記(6)で得られたサンプルを無アルカリガラス板(コーニング株式会社製「Eagle−XG」)に貼着した後、オートクレーブ中、温度50℃、圧力5MPaの条件下で20分間加圧処理を行ない、引き続き温度23℃、相対湿度60%の雰囲気下で1日放置した。その後、株式会社エスペック製の冷熱衝撃試験器「TSA−301L−W」にて、低温側−40℃〔保持時間30分〕、常温23℃〔保持時間5分〕、高温側85℃〔保持時間30分〕の順で試験槽ないが変化するように設定した条件で12サイクル保存する耐久性試験を行なった。その後、サンプルを取り出し、クラック状の外観不具合の有無を確認した。
After the sample obtained in (6) above is attached to a non-alkali glass plate (“Eagle-XG” manufactured by Corning Inc.), pressure treatment is performed for 20 minutes in an autoclave under the conditions of a temperature of 50 ° C. and a pressure of 5 MPa. Then, the mixture was allowed to stand for one day in an atmosphere having a temperature of 23 ° C. and a relative humidity of 60%. After that, using a cold shock tester "TSA-301L-W" manufactured by ESPEC CORPORATION, the low temperature side was -40 ° C [holding time 30 minutes], the room temperature was 23 ° C [holding
(8)実施例及び比較例
以下、上記(1)〜(6)の実施手順に従って作製した偏光板について、「(7)ヒートショック試験」を実施した結果を示す。
(8) Examples and Comparative Examples The following shows the results of performing "(7) heat shock test" on the polarizing plates prepared according to the procedures of (1) to (6) above.
[実施例1]
偏光フィルムのサイズが保護フィルムのサイズよりも縦方向及び横方向の全幅がいずれも0.1mm小さくなるように切り出し、各辺において偏光フィルムの端部が保護フィルムの端部に対して、それぞれ0.05mm内側に位置するように調整して、水系接着剤を使用して偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムのクラックは見られなかった。
[Example 1]
Cut out so that the size of the polarizing film is 0.1 mm smaller in both the vertical and horizontal directions than the size of the protective film, and the edge of the polarizing film is 0 on each side with respect to the edge of the protective film. A polarizing plate was prepared using an aqueous adhesive, adjusted to be located inside .05 mm, and a heat shock test was carried out. As a result, no cracks were observed in the polarizing film.
[実施例2]
偏光フィルムのサイズが保護フィルムのサイズよりも縦方向及び横方向の全幅がいずれも0.1mm小さくなるように切り出し、各辺において偏光フィルムの端部が保護フィルムの端部に対して、それぞれ0.05mm内側に位置するように調整して、カチオン系紫外線硬化性接着剤を使用して偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムのクラックは見られなかった。
[Example 2]
The size of the polarizing film is cut out so that the total width in the vertical direction and the horizontal direction is 0.1 mm smaller than the size of the protective film, and the edge of the polarizing film is 0 on each side with respect to the edge of the protective film. A polarizing plate was prepared using a cationic ultraviolet curable adhesive, adjusted to be located inside .05 mm, and a heat shock test was carried out. As a result, no cracks were observed in the polarizing film.
[実施例3]
偏光フィルムのサイズが保護フィルムのサイズよりも縦方向及び横方向の全幅がいずれも0.1mm小さくなるように切り出し、各辺において偏光フィルムの端部が保護フィルムの端部に対して、それぞれ0.05mm内側に位置するように調整して、ラジカル系紫外線硬化性接着剤を使用して偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムのクラックは見られなかった。
[Example 3]
The size of the polarizing film is cut out so that the total width in the vertical direction and the horizontal direction is 0.1 mm smaller than the size of the protective film, and the edge of the polarizing film is 0 on each side with respect to the edge of the protective film. A polarizing plate was prepared using a radical ultraviolet curable adhesive, adjusted to be located inside .05 mm, and a heat shock test was carried out. As a result, no cracks were observed in the polarizing film.
[実施例4]
保護フィルムをケン化処理したトリアセチルセルロース(コニカミノルタオプト株式会社製、ゼロタック、厚さ20μm)を使用したこと以外は実施例1と同様にして偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムのクラックは見られなかった。
[Example 4]
A polarizing plate was prepared in the same manner as in Example 1 except that triacetyl cellulose (manufactured by Konica Minolta Opto Co., Ltd., zero tack, thickness 20 μm) obtained by saponifying the protective film was used, and a heat shock test was carried out. As a result, no cracks were observed in the polarizing film.
[実施例5]
保護フィルムをケン化処理したトリアセチルセルロース(コニカミノルタオプト株式会社製、ゼロタック、厚さ20μm)を使用したこと以外は実施例2と同様にして偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムのクラックは見られなかった。
[Example 5]
A polarizing plate was prepared in the same manner as in Example 2 except that triacetyl cellulose (manufactured by Konica Minolta Opto Co., Ltd., zero tack, thickness 20 μm) obtained by saponifying the protective film was used, and a heat shock test was carried out. As a result, no cracks were observed in the polarizing film.
[実施例6]
保護フィルムをケン化処理したトリアセチルセルロース(コニカミノルタオプト株式会社製、ゼロタック、厚さ20μm)を使用したこと以外は実施例3と同様にして偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムのクラックは見られなかった。
[Example 6]
A polarizing plate was prepared in the same manner as in Example 3 except that triacetyl cellulose (manufactured by Konica Minolta Opto Co., Ltd., zero tack, thickness 20 μm) obtained by saponifying the protective film was used, and a heat shock test was carried out. As a result, no cracks were observed in the polarizing film.
[比較例1]
偏光フィルムと保護フィルムをいずれも130mm×80mmで切り出し、水系接着剤を使用して偏光板を作製したのち、スーパーカッターで各辺を5mmずつ裁断し、120mm×70mmに成形し、ヒートショック試験を実施した。その結果、偏光フィルムの端部にクラックが発生した。
[Comparative Example 1]
Both the polarizing film and the protective film are cut out to a size of 130 mm × 80 mm, a polarizing plate is prepared using an aqueous adhesive, and then each side is cut by 5 mm with a super cutter, molded into 120 mm × 70 mm, and subjected to a heat shock test. Carried out. As a result, cracks were generated at the edges of the polarizing film.
[比較例2]
偏光フィルムと保護フィルムをいずれも130mm×80mmで切り出し、カチオン系紫外線硬化性接着剤を使用して偏光板を作製したのち、スーパーカッターで各辺を5mmずつ裁断し、120mm×70mmに成形し、ヒートショック試験を実施した。その結果、その結果、偏光フィルムの端部にクラックが発生した。
[Comparative Example 2]
Both the polarizing film and the protective film were cut out to a size of 130 mm × 80 mm, a polarizing plate was prepared using a cationic ultraviolet curable adhesive, and then each side was cut by 5 mm with a super cutter and molded into 120 mm × 70 mm. A heat shock test was performed. As a result, cracks were generated at the edges of the polarizing film.
[比較例3]
偏光フィルムと保護フィルムをいずれも130mm×80mmで切り出し、ラジカル系紫外線硬化性接着剤を使用して偏光板を作製したのち、スーパーカッターで各辺を5mmずつ裁断し、120mm×70mmに成形し、ヒートショック試験を実施した。その結果、偏光フィルムの端部にクラックが多数発生した。
[Comparative Example 3]
Both the polarizing film and the protective film are cut out to a size of 130 mm × 80 mm, a polarizing plate is prepared using a radical ultraviolet curable adhesive, and then each side is cut by 5 mm with a super cutter and molded into 120 mm × 70 mm. A heat shock test was performed. As a result, many cracks were generated at the edges of the polarizing film.
[比較例4]
偏光フィルムのサイズが保護フィルムのサイズよりも縦方向及び横方向の全幅がいずれも0.1mm大きくなるように切り出し、各辺において、偏光フィルムの端部が保護フィルムの端部に対して、0.05mm外側に位置するように調整して、水系接着剤を使用して偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムの端部にクラックが発生した。
[Comparative Example 4]
The size of the polarizing film is cut out so that the total width in the vertical direction and the horizontal direction is 0.1 mm larger than the size of the protective film, and the edge of the polarizing film is 0 with respect to the edge of the protective film on each side. A polarizing plate was prepared using an aqueous adhesive, adjusted to be located .05 mm outside, and a heat shock test was carried out. As a result, cracks were generated at the edges of the polarizing film.
[比較例5]
偏光フィルムのサイズが保護フィルムのサイズよりも縦方向及び横方向の全幅がいずれも0.1mm大きくなるように切り出し、各辺において、偏光フィルムの端部が保護フィルムの端部に対して、0.05mm外側に位置するように調整して、カチオン系紫外線硬化性接着剤を使用して偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムの端部にクラックが発生した。
[Comparative Example 5]
The size of the polarizing film is cut out so that the total width in the vertical direction and the horizontal direction is 0.1 mm larger than the size of the protective film, and the edge of the polarizing film is 0 with respect to the edge of the protective film on each side. A polarizing plate was prepared using a cationic ultraviolet curable adhesive, adjusted to be located .05 mm outside, and a heat shock test was carried out. As a result, cracks were generated at the edges of the polarizing film.
[比較例6]
偏光フィルムのサイズが保護フィルムのサイズよりも縦方向及び横方向の全幅がいずれも0.1mm大きくなるように切り出し、各辺において、偏光フィルムの端部が保護フィルムの端部に対して、0.05mm外側に位置するように調整して、ラジカル系紫外線硬化性接着剤を使用して偏光板を作製し、ヒートショック試験を実施した。その結果、偏光フィルムの端部にクラックが多数発生した。
[Comparative Example 6]
The size of the polarizing film is cut out so that the total width in the vertical direction and the horizontal direction is 0.1 mm larger than the size of the protective film, and the edge of the polarizing film is 0 with respect to the edge of the protective film on each side. A polarizing plate was prepared using a radical ultraviolet curable adhesive, adjusted to be located .05 mm outside, and a heat shock test was carried out. As a result, many cracks were generated at the edges of the polarizing film.
本発明は、例えば液晶パネルの構成部品として利用することができる。 The present invention can be used, for example, as a component of a liquid crystal panel.
1A,1B,1C…偏光板、2…偏光フィルム(偏光子)、2a…偏光フィルムの端部、3…保護フィルム、3a…保護フィルムの端部、4…接着剤層(接着剤)、5…粘着剤層、6…反射型偏光子(光学機能フィルム)、8…液晶セル、9…液晶パネル、10…液晶表示装置。 1A, 1B, 1C ... polarizing plate, 2 ... polarizing film (polarizer), 2a ... edge of polarizing film, 3 ... protective film, 3a ... end of protective film, 4 ... adhesive layer (adhesive), 5 ... Adhesive layer, 6 ... Reflective polarizer (optical functional film), 8 ... Liquid crystal cell, 9 ... Liquid crystal panel, 10 ... Liquid crystal display device.
Claims (4)
前記偏光子は、厚さが10μm以下であり、
前記保護フィルムは、所定の形状に成形されたものであり、
前記保護フィルムは、前記偏光子の片面の全面に積層されており、
前記偏光子の全ての端部が、前記保護フィルムの端部よりも50〜500μm内側に位置しており、
前記偏光子における前記保護フィルムが積層されている側とは反対側の面、及び、前記保護フィルムにおける前記偏光子が積層されている側とは反対側の面の少なくとも一方の面に積層された粘着剤層を更に備え、
前記粘着剤層を介して積層された反射型偏光子を更に備える、偏光板。 It comprises a polarizer and a protective film laminated on only one side thereof with an adhesive.
The polarizer has a thickness of 10 μm or less and has a thickness of 10 μm or less.
The protective film is formed into a predetermined shape and has a predetermined shape.
The protective film is laminated on the entire surface of one side of the polarizer.
All ends of the polarizer are located 50 to 500 μm inside the edges of the protective film .
It was laminated on at least one surface of the protector opposite to the side on which the protective film was laminated and on the surface of the protective film opposite to the side on which the protector was laminated. With an additional adhesive layer,
A polarizing plate further comprising a reflective polarizing element laminated via the pressure-sensitive adhesive layer .