JP4357379B2 - インクジェット記録媒体の製造方法 - Google Patents
インクジェット記録媒体の製造方法 Download PDFInfo
- Publication number
- JP4357379B2 JP4357379B2 JP2004201492A JP2004201492A JP4357379B2 JP 4357379 B2 JP4357379 B2 JP 4357379B2 JP 2004201492 A JP2004201492 A JP 2004201492A JP 2004201492 A JP2004201492 A JP 2004201492A JP 4357379 B2 JP4357379 B2 JP 4357379B2
- Authority
- JP
- Japan
- Prior art keywords
- inorganic fine
- fine particle
- coating
- particle layer
- silica
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Description
[Al(OH)3]nAlCl3 一般式2
Aln(OH)mCl(3n-m) 0<m<3n 一般式3
低密度ポリエチレン 30部
(密度0.920g/cm3)
高密度ポリエチレン 70部
(密度0.967g/cm3)
<表樹脂配合>
マスターバッチ 15部
(密度0.918g/cm3の低密度ポリエチレン39.1部、Al2O3換算0.8質量%の表面被覆アナタ−ゼ型酸化チタン60部、ステアリン酸亜鉛0.9部をバンバリーミキサーで混練)
低密度ポリエチレン 85部
(密度0.920g/cm3)
<バックコート塗液配合>
無水マレイン酸重合体のアルカリ加水分解物25%液 4部
コロイド状シリカ20%スラリー
(日産化学工業(株)製スノーテックス20) 20部
エポキシタイプ架橋剤10%液 1.5部
スルフォコハク酸−2−エチルヘキシルエステル塩5%液 0.5部
水にて全量を100部とした。
<下引き液配合>
石灰処理ゼラチン2%水溶液 50部
スルフォコハク酸−2−エチルヘキシルエステル塩5%液 0.5部
クロム明ばん5%水溶液 2部
水にて全量を100部とした。
<多孔質層塗布液配合1>
気相法シリカ20%スラリー 70部
(平均一次粒径12nm)
ポリジメチルアリルアンモニウムクロライド10%水溶液 2.8部
硼酸10%水溶液 4.2部
ポリビルアルコール10%水溶液 21部
(鹸化度88%、平均重合度3500)
界面活性剤5%水溶液 0.84部
水にて全量を100部とした。
<無機微粒子層塗布液配合1>
コロイド状シリカ20%スラリー 8部
(日産化学工業(株)製スノーテックスO;平均一次粒径15nm)
水にて全量を100部とした。(シリカ濃度1.6質量%)
粘度は1.3mPa・sであった。
(算定厚み187nm:湿分塗布量(19ml/m2)×塗布液濃度(0.016)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
<無機微粒子層塗布液配合2>
コロイド状シリカ20%スラリー 6部
(日産化学工業(株)製スノーテックスO;平均一次粒径15nm)
水にて全量を100部とした。(シリカ濃度1.2質量%)
粘度は1.3mPa・sであった。
(算定厚み140nm:湿分塗布量(19ml/m2)×塗布液濃度(0.012)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
<無機微粒子層塗布液配合3>
コロイド状シリカ20%スラリー 4部
(日産化学工業(株)製スノーテックスO;平均一次粒径15nm)
水にて全量を100部とした。(シリカ濃度0.8質量%)
粘度は1.3mPa・sであった。
(算定厚み93nm:湿分塗布量(19ml/m2)×塗布液濃度(0.008)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
実施例1の無機微粒子層塗布液配合を無機微粒子層塗布液配合4に代える以外は同様にして比較例1のインクジェット記録媒体を得た。
<無機微粒子層塗布液配合4>
コロイド状シリカ20%スラリー 20部
(日産化学工業(株)製スノーテックスO;平均一次粒径15nm)
水にて全量を100部とした。(シリカ濃度4.0質量%)
粘度は1.3mPa・sであった。
(算定厚み477nm:湿分塗布量(19ml/m2)×塗布液濃度(0.04)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
実施例3に於いて無機微粒子層塗布液の塗布量を30ml/m2にする以外は同様にして比較例2のインクジェット記録媒体を得た。
(算定厚み147nm:湿分塗布量(30ml/m2)×塗布液濃度(0.008)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
(算定厚み147nm:湿分塗布量(20ml/m2)×塗布液濃度(0.012)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
(算定厚み98nm:湿分塗布量(20ml/m2)×塗布液濃度(0.008)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
実施例4の無機微粒子層塗布液配合を無機微粒子層塗布液配合4に代える以外は同様にして比較例3のインクジェット記録媒体を得た。
(算定厚み502nm:湿分塗布量(20ml/m2)×塗布液濃度(0.04)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
<無機微粒子層塗布液配合5>
コロイド状シリカ20%スラリー 6部
(扶桑化学工業製クォートロンPL−3L、平均一次粒径35nm)
水にて全量を100部とした。(シリカ濃度1.2質量%)
粘度は1.3mPa・sであった。
(算定厚み147nm:湿分塗布量(20ml/m2)×塗布液濃度(0.012)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
<無機微粒子層塗布液配合6>
コロイド状シリカ20%スラリー 4部
(扶桑化学工業製クォートロンPL−3L、平均一次粒径35nm)
水にて全量を100部とした。(シリカ濃度0.8質量%)
粘度は1.3mPa・sであった。
(算定厚み98nm:湿分塗布量(20ml/m2)×塗布液濃度(0.008)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
実施例4の無機微粒子層塗布液配合を無機微粒子層塗布液配合7に代える以外は同様にして比較例4のインクジェット記録媒体を得た。
<無機微粒子層塗布液配合7>
コロイド状シリカ20%スラリー 20部
(日産化学工業(株)製スノーテックスO;平均一次粒径15nm)
水にて全量を100部とした。(シリカ濃度4.0質量%)
(算定厚み502nm:湿分塗布量(20ml/m2)×塗布液濃度(0.04)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
<無機微粒子層塗布液配合8>
コロイド状シリカ12%スラリー 10部
(扶桑化学工業製クォートロンPL−1、平均一次粒径15nm)
水にて全量を100部とした。(シリカ濃度1.2質量%)
粘度は1.3mPa・sであった。
(算定厚み147nm:湿分塗布量(20ml/m2)×塗布液濃度(0.012)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
<無機微粒子層塗布液配合9>
コロイド状シリカ12%スラリー 6.7部
(扶桑化学工業製クォートロンPL−1、平均一次粒径15nm)
水にて全量を100部とした。(シリカ濃度0.8質量%)
(算定厚み98nm:湿分塗布量(20ml/m2)×塗布液濃度(0.008)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
実施例4の無機微粒子層塗布液配合を無機微粒子層塗布液配合10に代える以外は同様にして比較例5のインクジェット記録媒体を得た。
<無機微粒子層塗布液配合10>
コロイド状シリカ12%スラリー 33部
(扶桑化学工業製クォートロンPL−1、平均一次粒径15nm)
水にて全量を100部とした。(シリカ濃度4.0質量%)
(算定厚み502nm:湿分塗布量(20ml/m2)×塗布液濃度(0.04)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
なお、実施例1〜9及び比較例1〜4の無機微粒子層塗液の吸収所要時間は何れも0.3秒以内であった。
実施例9の塗布方法をアプリケーターロールで塗布液を供給後、エアナイフで掻き落として塗布量を調節する後計量タイプの塗布方式に変更して比較例6のインクジェット記録媒体を得た。湿分塗布量は塗布中における単位時間当たりの塗液減少量から計算された。
(算定厚み88nm:湿分塗布量(18ml/m2)×塗布液濃度(0.008)÷二酸化珪素の密度(2.2g/cm3)÷0.74)
実施例1の無機微粒子層塗布前の試料を比較例7のインクジェット記録媒体とした。
これらインクジェット記録媒体は、密封包装のもと50℃24時間経時後、以下の評価を行った。
<インク吸収性>
インクジェット記録媒体を23℃、湿度55%RHに一昼夜調湿後、同条件下でセイコーエプソン社製インクジェットプリンターMJ−800Cで黒ベタ印字後、時間間隔を変化して印字面にPPC用紙を重ねて軽く圧着し、剥がしてPPC用紙へのインク裏写りを評価した。
◎;20秒後でも全く裏写り無し。
○;20秒後ではやや裏写り有るが、25秒後では全く裏写り無し。
△;25秒後ではやや裏写り有るが、30秒後では全く裏写り無し。
×;30秒後でも裏写りが有る
インクジェット記録媒体の印字していない部分の光沢を目視で判定した。
○;写真用印画紙並で非常に良好。
△;アート、コート紙のレベルで良好。
×;マット紙に近く大幅に悪い。
インクジェット記録媒体の観察角度を変えながら干渉縞の見え方を分類した。
○;十分に傾けて干渉縞を探すと見える。
△;普通は見えないが大きく傾けた時、干渉縞が見える。
×;通常の観察角度の範囲でも干渉縞が見えることが有る。
また、表中「−」は無機微粒子層が無いか、表面の乱れのため光沢が無く、干渉縞の評価が出来ないことを表す。
外観上の故障の有無を観察した。以上結果を表1に示す。
Claims (1)
- 支持体上に、少なくとも1層の、平均二次粒子径が500nm以下のシリカ微粒子を含有する多孔質層を形成した後に、該多孔質層の上に無機微粒子層を設けるインクジェット記録媒体の製造方法であって、該多孔質層を形成した後に該無機微粒子層の塗布液を塗布するに際し、該無機微粒子層の塗布液は無機微粒子として球状のコロイド状シリカを含有し、且つ該無機微粒子層の塗布液の35℃粘度が10mPa・S以下であって、該多孔質層の空隙容量の90容量%以下の塗布量で、前計量タイプの塗布方式として直径100mm以下の斜線グラビアロールをリバース且つキスタッチにて使用する塗布装置にて塗布して、無機微粒子の固形分塗布量が0.304g/m2以下の無機微粒子層を設けることを特徴とするインクジェット記録媒体の製造方法。