JP3652915B2 - Corrosion-resistant coating forming method on inner surface of cylindrical container and apparatus for forming the same - Google Patents
Corrosion-resistant coating forming method on inner surface of cylindrical container and apparatus for forming the same Download PDFInfo
- Publication number
- JP3652915B2 JP3652915B2 JP07463699A JP7463699A JP3652915B2 JP 3652915 B2 JP3652915 B2 JP 3652915B2 JP 07463699 A JP07463699 A JP 07463699A JP 7463699 A JP7463699 A JP 7463699A JP 3652915 B2 JP3652915 B2 JP 3652915B2
- Authority
- JP
- Japan
- Prior art keywords
- cylindrical container
- corrosion
- resistant coating
- frequency heating
- container
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
【0001】
【発明の属する技術分野】
本発明は、ナトリウム二次電池の外筒容器等を構成する円筒容器内面への耐食被覆形成方法及びその形成装置に関するものである。
【0002】
【従来の技術】
従来のナトリウム二次電池は、硫黄(S)を含む正極活物資と、ナトリウムを含む負極活物資と、ナトリウムイオンに対して伝導性を有する固体電解質管と、正極端子である円筒缶状の外筒容器と、絶縁リングと、負極端子である封口蓋とを備えている。そして、外筒容器には、正極活物資と中空円筒状導電助材が収納され、該導電助材の中空部には固体電解質管が挿入され、該固体電解質管には負極活物資であるナトリウムが収納されている。
【0003】
このナトリウム二次電池の放電時には、ナトリウムイオンと硫黄とが反応して腐食性の高い多硫化ナトリウム(Na2Sx)を生成し、該多硫化ナトリウムが硫黄中に拡散することになる。したがって、外筒容器の内面は、電池の放電時等に硫黄あるいは多硫化ナトリウムに曝され、厳しい腐食環境下にある。
そこで、従来におけるナトリウム二次電池の外筒容器の内面には、メッキ又は溶射により耐食被覆が形成され、防食対策が施されている。なお、耐食被覆の材質としては、耐腐食性が高いFe―Cr系合金等が用いられている。
【0004】
【発明が解決しようとする課題】
しかしながら、上述した従来の耐食被覆形成方法では、外筒容器の内面全体にわたって厚さが均一な耐食被覆を形成することは困難であり、また、外筒容器の内面に対する耐食被覆の密着性も低いので、耐食被覆にクラックが生じたり、あるいは耐食被覆が外筒容器の内面から剥離したりすることが起こり、多硫化ナトリウムと外筒容器の内面が接触して該外筒容器が腐食されてしまうという不具合があった。
なお、耐食被覆の形成方法としては、メッキ法や溶射法が主流であるが、低コスト化及び信頼性向上の観点から、基材に合金粉末を溶射あるいは塗布し溶融処理を施してコーティングする粉体融着方式も考えられる。即ち、母材表面に配した自溶性合金等の粉体を、バーナ加熱あるいは高周波加熱で1000℃を超える高温で溶融させ、凝固させて融着させるものいであるが、ナトリウム二次電池の外筒容器のように、胴部と底部を分けるコーナー部において状況が一変する部材に対して、気孔のない緻密な被覆を、クラックなしで形成するのは至難と思われた。
【0005】
本発明はこのような実状に鑑みてなされたものであって、その目的は、円筒容器の内面に対する密着性が高く、かつ均一な厚さの信頼性の高い耐食被覆を形成すると共に、溶融処理を高速で行い、生産能率の向上を図ることが可能な円筒容器内面の耐食被覆形成方法及びその形成装置を提供することにある。
【0006】
【課題を解決するための手段】
上記従来技術の有する課題を解決するために、本発明の円筒容器内面への耐食被覆形成方法においては、金属製の円筒容器の内面に、耐食合金の粉体を、層状に配置し、次いで、該容器を回転させながら、容器の胴部に移動方式の高周波加熱を適用して胴部内面の粉体を開口端から底部端に向けて順次溶融させて行くとともに、胴部の加熱が底部端に達する迄の選定された時期に底部の高周波加熱を開始して、胴部加熱の底部端到達と同時に底部の加熱を終了させ円筒容器内面へ耐食被覆を形成させる。
【0007】
また、本発明の円筒容器内面への耐食被覆形成装置においては、内面に円筒容器を回転自在に支持する支持手段と、前記円筒容器の胴部の周囲に配設されて該胴部を加熱する第1の高周波加熱コイルと、前記円筒容器の底部外面近傍に配設されて該底部を加熱する第2の高周波加熱コイルと、前記第1と第2の高周波加熱コイルに通電するための高周波電源とを備えている。
【0008】
【発明の実施の形態】
以下、本発明を図示の実施の形態に基づいて詳細に説明する。
【0009】
図1及び図2は、本発明に係る円筒容器内面の耐食被覆形成方法及びその形成装置の実施形態を示している。図における円筒容器1は、一端が開口した胴部2と、該胴部2の他端に設けられた底部3とから構成される円筒缶状の底付き容器である。この円筒容器1は、図2に示すようなナトリウム二次電池の正極外筒容器として使用され、円筒容器1の内面1aには耐食被覆4が形成されている。
円筒容器1は、炭素鋼、低合金鋼、ステンレス鋼、Ni系合金等からなる材料を用いて成形加工されている。また、耐食被覆4は、Ni,Crを主成分とし、自溶性をもたらすフラックス生成成分B,Siが配合されており、加熱溶融させることが気孔をなくして緻密化するとともに下地金属に融着させるための溶融処理が特に容易に行えるNi系(Ni−Cr系とも呼ばれる)の自溶合金を用いて形成されている。この自溶合金は、Ni,Cr等の耐食性金属を主成分として含んでいるので、300〜350℃の環境下で多硫化ナトリウム及び硫黄に対する耐腐食性が高く、耐食被覆4の材質として好ましい上、耐食被覆4を容易に形成することが可能である。Co系自溶合金についても同様である。
【0010】
上記耐食被覆4は、図1に示すような耐食被覆形成装置5を用いて円筒容器1の内面1aに形成されている。この形成装置5は、内面1aに耐食合金の自溶合金が溶射法、スラリー塗動法、遠心焼結法または遠心配置法によって層状に配置された円筒容器1を回転自在に支持する支持手段6と、円筒容器1の胴部2の周囲に移動可能に配設され、胴部2を加熱する第1高周波加熱コイル(胴部高周波加熱コイル)7と、円筒容器1の底部3の外側近傍に配設され、底部3を加熱する第2高周波加熱コイル(底部高周波加熱コイル)8と、これら第1及び第2高周波加熱コイル7,8の高周波加熱電源(図示せず)と、図示しないトランスフォーマ(変圧器)と、Ar,N2等の不活性ガスを円筒容器1の内面1aに導入するガスノズル9とをそれぞれ備えている。
【0011】
上記支持手段6は、図示しない旋盤の主軸などに回転可能に取付けられるチャック(回転台)10と、基端が当該チャック10に装着される容器取付治具11とを備えており、円筒容器1は、胴部2の開口側を容器取付治具11の先端内部に挿入してボルト締めすることにより、支持手段6を介して旋盤の主軸などに回転自在に支持されるようになっている。
【0012】
また、上記第1高周波加熱コイル7は、内径が円筒容器1の胴部2の外径よりも大きなリング状(他の形状でもよい)に形成され、円筒容器1の胴部2に遊嵌された状態で配置されている。しかも、第1高周波加熱コイル7は、図示しない移動装置に取付けられており、この移動装置によりチャック10側から底部3の付近まで円筒容器1の胴部2を軸方向へ沿って加熱しながら移動できるように構成されている。
さらに、上記第2高周波加熱コイル8は渦巻状コイルを用いて形成されている。しかも、第2高周波加熱コイル8は、図示しない支持装置に取付けられており、該支持装置にて円筒容器1の軸心より偏心した位置に配設され、容器を回転させたときに該円筒容器1の底部3が均一に加熱されるようになっている。なお、第1及び第2高周波加熱コイル7,8は、ケーブル,トランスフォーマなどを介して高周波加熱電源(いずれも図示せず)に接続されている。
【0013】
一方、上記ガスノズル9は、支持手段6のチャック10及び容器取付治具11を経て円筒容器1内の底部3の付近まで貫通配置されている。そして、ガスノズル9の一端は、図示しないAr,N2等の不活性ガス供給源に連結されており、自溶合金の酸化防止のため、このガス供給源から送られた不活性ガスを先端より円筒容器1の内面1a全体に供給するように構成されている。したがって、ガスノズル9は、自溶合金が酸化し易い材料の時のみ必要であって、酸化しにくい材料の場合には不要である。
【0014】
次に、本発明の実施形態の耐食被覆形成装置5を用いて円筒容器1の内面1aに耐食被覆4を形成する耐食被覆形成方法を説明する。
まず、本発明に用いる耐食合金の平均粒径は、10〜300μmの範囲内であるのが好ましい。これは、平均粒径10μm未満では、小さい粒子同士が結合して形状が不均一な粗大粒子が形成されることになり、また平均粒径が300μmを越えると、スラリー化したときに粉末が沈殿してしまうなどの支障が生じるので好ましくないからである。
そして、耐食被覆4の原料粉末とバインダー等とを混合してスラリー状の塗布剤を調製し、この調製した塗布剤を円筒容器1の内面1aに均一に塗布する。また、溶射皮膜の場合は、プラズマ溶射機、高速燃焼炎溶射機、フレーム溶射機などの溶射機で上記原料粉末を溶解して円筒容器1の内面1aに均一に吹き付けて溶射する。さらに遠心焼結法または遠心配置法による場合は円筒容器1の内面1aの下部に均一に分散させる。
ここで遠心焼結法とは、容器内に粉体を軸方向均等に挿入し、回転により周方向にも均等化させ、遠心力で胴部内面に留まった状態で融点未満の加熱で焼結させる手法を、又、遠心配置法とは容器内に粉体を軸方向均等に装入し、回転により周方向にも均等化させ遠心力で胴部内面に留まらせておく手法をそれぞれ指すものとする。
【0015】
次いで、図1に示す如く、内面1aに耐食合金が溶射法、スラリー塗布法、遠心焼結法または円筒容器1の開口側を支持手段6の容器取付治具11を介して旋盤の主軸などに取付け、回転させる。このように、円筒容器1を回転させるのは、溶融処理時に気孔を低減させるために実施するものである。
この状態で、第1高周波加熱コイル7を支持手段6のチャック10側から円筒容器1の胴部2に沿って軸方向へ移動させることにより当該胴部2を加熱する。そして、第1高周波加熱コイル7が円筒容器1の底部3の近傍に移動したとき、第2高周波加熱コイル8の加熱を開始して円筒容器1の底部3を加熱する。これにより、円筒容器1の全体が加熱され、第1の高周波加熱コイル7が胴部2の底部端のコーナー部までの溶融を終える時点で底部3内面の粉体を過不足のない温度の溶融状態に到達させるよう第2高周波加熱コイル8の加熱開始時期を選定することにより、胴部2と底部3の粉体の溶融がコーナー部において熱的に同等の状態で同時に終了するところとなって、この円筒容器1の内面1aの全面に、耐食被覆4が、どの部位にも大きな熱応力を残さずに形成されることになる(図2参照)。この耐食被覆4の厚さは、10μm以上1000μm以下、好ましくは50〜100μmの範囲内であることが良い。厚さが10μm未満では、耐食被覆4が薄すぎて円筒容器1の内面1aが多硫化ナトリウムにより腐食されるおそれがあり、厚さが1000μmを超えると、応力の累積などによって剥がれやすくなり、好ましくないからである。
なお、加熱中は円筒容器1の全体を常時回転させておく。そして、加熱温度は、1030〜1200℃の範囲内であることが好ましい。加熱温度が1030℃未満では、温度が低すぎて耐食被覆4の原料粉末を融点以上まで加熱できず、1200℃を越えると、円筒容器1の強度が低下してしまい、好ましくないからである。また、自溶合金の酸化防止の観点から、不活性ガスをガスノズル10より円筒容器1の内面1aに導入し、円筒容器1の内部を不活性ガス雰囲気にしておくことが好ましい。
【0016】
ここで、本発明の実施形態に係る耐食被覆形成方法及び耐食被覆形成装置5によって、円筒容器1の内面1aに施された溶射皮膜から耐食被覆4を形成することが可能であるか否かの試験を行った。
供試体としては、ステンレス鋼(SUS304)からなり、外径60mm、肉厚1.5mm、長さ400mmに成形加工された円筒容器を用い、その内面には耐食合金の溶射皮膜が施されている。また、耐食被覆形成装置5は、下記の表1で示す試験条件の下、胴部移動加熱をチャック側より開始し、予め設定した底部加熱時間と移動加熱の終了時間が同時になるように、底部加熱を開始した。
【0017】
【表1】
【0018】
このような試験を実施して熱電対による円筒容器の各部の温度測定を行うと、胴部全長の1/2位置近傍では1065℃、底部中心位置では1075℃、底部エッヂでは1035℃という結果が得られた。また、移動加熱した胴部の温度差は±20℃の範囲であり、底部はコイルを40mm偏心させた状態で、エッヂ部昇温までに77秒を要した。しかも、底部の中心とエッヂ部の温度差は40℃と好結果が得られた。
したがって、円筒容器の内面に施された溶射皮膜の溶融処理は、今回試験の加熱方法により施工可能であり、本発明の実施形態に係る耐食被覆形成方法及び耐食被覆形成装置5によって、円筒容器1の内面1aに耐食被覆4を形成し得ると判断できる。
【0019】
このように、本発明の実施形態に係る耐食被覆形成方法にあっては、内面1aに耐食合金が塗布溶射又は挿入されて均一に分散され、耐食被覆形成装置5の支持手段6に支持された円筒容器1を図外の旋盤の主軸などで回転させながら、第1高周波加熱コイル7を円筒容器1に沿って軸方向へ移動させることにより、円筒容器1の胴部2を加熱すると共に、第1高周波加熱コイル7が円筒容器1の底部3の近傍に移動したとき、第2高周波加熱コイル8の加熱を開始して円筒容器1の底部3を加熱しており、これにより円筒容器1の全体を加熱して該円筒容器1の内面1aに耐食被覆4を形成しているため、簡単な構造の形成装置5で円筒容器1に対して加熱温度を均一にすることが可能となる。したがって、本実施形態の形成方法によれば、内面1aに均一な厚さであっても、どの部位にも大きな熱応力が残留していない4が形成された信頼性の高い円筒容器1を得ることができる。
また、本実施形態の第2高周波加熱コイル8は、円筒容器1の底部3の外側近傍で、円筒容器1の軸心より偏心した位置に配設されているため、当該円筒容器1の底部3をより一層均一に加熱することができる。
【0020】
以上、本発明の実施の形態につき述べたが、本発明は既述の実施の形態に限定されるものではなく、本発明の要旨を逸脱しない範囲内において種々の変形及び変更を加え得るものである。
例えば、円筒容器1は、ナトリウム二次電池の正極外筒容器以外の円筒容器にも使用できる。また、耐食合金の原料粉末が酸化しにくい材料である場合には、円筒容器1内にガスノズル9を貫通配置する必要がない。
【0021】
【発明の効果】
上述した如く、本発明に係る円筒容器内面の耐食被覆形成方法は、内面に耐食合金が塗布又は溶射された円筒容器を回転させ、この状態で第1高周波加熱コイルを前記円筒容器に沿って移動させることにより前記円筒容器の胴部を加熱し、次いで、前記第1高周波加熱コイルが前記円筒容器の底部近傍に移動したとき、第2高周波加熱コイルの加熱を開始して前記円筒容器の底部を加熱して胴部と底部の加熱が同時に終了するようにし、これにより円筒容器全体を準一方向的に加熱しひいては凝固させて前記円筒容器の内面に耐食被覆を形成しているので、円筒容器の内面に対する密着性が高く緻密であり、かつ均一な厚さと性状を有する残留応力の小さい耐食被覆を確実に形成でき、製品の信頼性向上を図ることができる。
【0022】
また、他の本発明に係る円筒容器内面の耐食被覆形成装置は、内面に耐食合金、溶射法、スラリー塗布法、遠心焼結法、または遠心配置法によって施工された円筒容器を回転自在に支持する支持手段と、前記円筒容器の胴部の周囲に移動可能に配設され、該胴部を加熱する第1高周波加熱コイルと、前記円筒容器の底部の外側近傍に配設され、該底部を加熱する第2高周波加熱コイルと、前記第1及び第2高周波加熱コイルの高周波加熱電源とをそれぞれ備えているので、上記発明と同様の効果が得られる上、簡単な構造で溶融処理を高速で行い、生産能率を向上させることができる。
【図面の簡単な説明】
【図1】本発明の実施形態に係る円筒容器内面の耐食被覆形成方法を説明するものであって、その方法で使用される耐食被覆形成装置を概念的に示す側面図である。
【図2】本発明の実施形態に係る耐食被覆形成方法により得られた円筒容器を示す断面図である。
【符号の説明】
1 円筒容器
1a 円筒容器の内面
2 胴部
3 底部
4 耐食被覆
5 耐食被覆形成装置
6 支持手段
7 第1高周波加熱コイル
8 第2高周波加熱コイル
9 ガスノズル
10 チャック
11 容器取付治具[0001]
BACKGROUND OF THE INVENTION
The present invention relates to a method and apparatus for forming a corrosion-resistant coating on the inner surface of a cylindrical container constituting an outer container or the like of a sodium secondary battery.
[0002]
[Prior art]
A conventional sodium secondary battery includes a positive electrode active material containing sulfur (S), a negative electrode active material containing sodium, a solid electrolyte tube having conductivity with respect to sodium ions, and a cylindrical can-shaped outer electrode serving as a positive electrode terminal. A cylindrical container, an insulating ring, and a sealing lid that is a negative electrode terminal are provided. The outer casing container contains a positive electrode active material and a hollow cylindrical conductive aid, a solid electrolyte tube is inserted into the hollow portion of the conductive aid, and the solid electrolyte tube has sodium as a negative electrode active material. Is stored.
[0003]
During discharge of the sodium secondary battery, sodium ions and sulfur react to generate highly corrosive sodium polysulfide (Na 2 Sx), and the sodium polysulfide diffuses into the sulfur. Therefore, the inner surface of the outer casing is exposed to sulfur or sodium polysulfide when the battery is discharged, and is in a severe corrosive environment.
Therefore, a corrosion-resistant coating is formed on the inner surface of the outer casing of the conventional sodium secondary battery by plating or spraying, and anti-corrosion measures are taken. As a material for the corrosion resistant coating, an Fe—Cr alloy or the like having high corrosion resistance is used.
[0004]
[Problems to be solved by the invention]
However, in the conventional corrosion-resistant coating forming method described above, it is difficult to form a corrosion-resistant coating having a uniform thickness over the entire inner surface of the outer cylinder container, and the adhesion of the corrosion-resistant coating to the inner surface of the outer cylinder container is low. As a result, the corrosion-resistant coating cracks or the corrosion-resistant coating is peeled off from the inner surface of the outer cylinder container, and sodium polysulfide and the inner surface of the outer cylinder container come into contact with each other and the outer cylinder container is corroded. There was a problem that.
As a method for forming a corrosion-resistant coating, a plating method or a thermal spraying method is the mainstream, but from the viewpoint of cost reduction and reliability improvement, a powder to be coated by spraying or applying an alloy powder to a base material and subjecting it to a melting treatment. A body fusion method is also conceivable. That is, a powder such as a self-fluxing alloy disposed on the surface of a base material is melted at a high temperature exceeding 1000 ° C. by burner heating or high-frequency heating, and solidified and fused. It seems that it is very difficult to form a dense coating without cracks on a member whose situation changes completely in a corner part that separates the body part and the bottom part like a container.
[0005]
The present invention has been made in view of such a situation, and an object thereof is to form a highly reliable corrosion-resistant coating having a high adhesion to the inner surface of the cylindrical container and a uniform thickness, and a melting treatment. It is an object of the present invention to provide a method and apparatus for forming a corrosion-resistant coating on the inner surface of a cylindrical container that can improve the production efficiency at a high speed.
[0006]
[Means for Solving the Problems]
In order to solve the above-described problems of the prior art, in the corrosion-resistant coating forming method on the inner surface of the cylindrical container of the present invention, the corrosion-resistant alloy powder is arranged in a layer on the inner surface of the metal cylindrical container, While rotating the container, the high frequency heating of the moving system is applied to the body of the container to melt the powder on the inner surface of the body sequentially from the opening end to the bottom end, and the heating of the body is performed at the bottom end. High frequency heating of the bottom is started at a selected time until reaching the bottom, and at the same time as the bottom end of the body heating is reached, the bottom heating is terminated and a corrosion-resistant coating is formed on the inner surface of the cylindrical container.
[0007]
Further, in the corrosion-resistant coating forming apparatus for the inner surface of the cylindrical container according to the present invention, the supporting means for rotatably supporting the cylindrical container on the inner surface and the periphery of the cylindrical portion of the cylindrical container are heated. A first high-frequency heating coil; a second high-frequency heating coil disposed near the outer surface of the bottom of the cylindrical container to heat the bottom; and a high-frequency power source for energizing the first and second high-frequency heating coils And.
[0008]
DETAILED DESCRIPTION OF THE INVENTION
Hereinafter, the present invention will be described in detail based on illustrated embodiments.
[0009]
1 and 2 show an embodiment of a method and apparatus for forming a corrosion-resistant coating on the inner surface of a cylindrical container according to the present invention. A
The
[0010]
The corrosion-resistant coating 4 is formed on the
[0011]
The support means 6 includes a chuck (rotary table) 10 that is rotatably attached to a main shaft of a lathe (not shown) and a container attachment jig 11 that has a base end attached to the
[0012]
The first high-frequency heating coil 7 is formed in a ring shape (other shape may be acceptable) whose inner diameter is larger than the outer diameter of the body portion 2 of the
Further, the second high frequency heating coil 8 is formed using a spiral coil. In addition, the second high-frequency heating coil 8 is attached to a support device (not shown), and is disposed at a position eccentric from the axial center of the
[0013]
On the other hand, the
[0014]
Next, a corrosion resistant coating forming method for forming the corrosion resistant coating 4 on the
First, the average particle diameter of the corrosion resistant alloy used in the present invention is preferably in the range of 10 to 300 μm. When the average particle size is less than 10 μm, small particles are bonded to each other to form coarse particles having a non-uniform shape. When the average particle size exceeds 300 μm, the powder precipitates when slurried. This is because it is not preferable because troubles such as the occurrence of trouble occur.
Then, the raw material powder of the corrosion-resistant coating 4 and a binder are mixed to prepare a slurry-like coating agent, and the prepared coating agent is uniformly applied to the
Here, the centrifugal sintering method means that the powder is inserted into the container evenly in the axial direction, and is also equalized in the circumferential direction by rotation, and sintered by heating below the melting point while remaining on the inner surface of the body by centrifugal force. In addition, the centrifugal arrangement method refers to a method in which powder is uniformly loaded in the container in the axial direction, and is also made uniform in the circumferential direction by rotation and kept on the inner surface of the body by centrifugal force. And
[0015]
Next, as shown in FIG. 1, a corrosion resistant alloy is sprayed onto the
In this state, the first high-frequency heating coil 7 is moved in the axial direction along the body 2 of the
In addition, the whole
[0016]
Here, whether or not the corrosion-resistant coating 4 can be formed from the sprayed coating applied to the
As a specimen, a cylindrical container made of stainless steel (SUS304) and molded to have an outer diameter of 60 mm, a wall thickness of 1.5 mm, and a length of 400 mm is used, and a thermal spray coating of a corrosion resistant alloy is applied to the inner surface thereof. . Further, the corrosion-resistant coating forming apparatus 5 starts torso moving heating from the chuck side under the test conditions shown in Table 1 below, so that the preset bottom heating time and moving heating end time are simultaneously set. Heating was started.
[0017]
[Table 1]
[0018]
When the temperature of each part of the cylindrical container was measured using a thermocouple after such a test, the results were 1065 ° C. near the half position of the entire body length, 1075 ° C. at the bottom center position, and 1035 ° C. at the bottom edge. Obtained. Further, the temperature difference of the body portion heated and moved was in the range of ± 20 ° C., and the bottom portion required 77 seconds to elevate the edge portion with the coil being eccentric by 40 mm. Moreover, the temperature difference between the center of the bottom and the edge was 40 ° C., and a good result was obtained.
Therefore, the melt treatment of the sprayed coating applied to the inner surface of the cylindrical container can be performed by the heating method of the test this time, and the
[0019]
Thus, in the corrosion-resistant coating forming method according to the embodiment of the present invention, the corrosion-resistant alloy is applied and sprayed or inserted on the
In addition, the second high-frequency heating coil 8 of the present embodiment is disposed near the outside of the bottom 3 of the
[0020]
Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, and various modifications and changes can be made without departing from the scope of the present invention. is there.
For example, the
[0021]
【The invention's effect】
As described above, the method for forming a corrosion-resistant coating on the inner surface of a cylindrical container according to the present invention rotates a cylindrical container whose inner surface is coated or sprayed with a corrosion-resistant alloy, and moves the first high-frequency heating coil along the cylindrical container in this state. To heat the body of the cylindrical container, and then when the first high-frequency heating coil moves to the vicinity of the bottom of the cylindrical container, heating of the second high-frequency heating coil is started and the bottom of the cylindrical container is moved. Since the heating of the body and the bottom is completed at the same time by heating, the entire cylindrical container is quasi-unidirectionally heated and solidified to form a corrosion-resistant coating on the inner surface of the cylindrical container. Therefore, it is possible to reliably form a corrosion-resistant coating having a high adhesiveness to the inner surface and having a uniform thickness and properties and a small residual stress, thereby improving the reliability of the product.
[0022]
In addition, the corrosion-resistant coating forming apparatus for the inner surface of a cylindrical container according to another aspect of the present invention rotatably supports a cylindrical container constructed on the inner surface by a corrosion-resistant alloy, a thermal spraying method, a slurry coating method, a centrifugal sintering method, or a centrifugal arrangement method. Supporting means, a first high-frequency heating coil that is movably disposed around the body of the cylindrical container, and is disposed in the vicinity of the outside of the bottom of the cylindrical container. Since the second high-frequency heating coil to be heated and the high-frequency heating power sources of the first and second high-frequency heating coils are provided, the same effects as the above invention can be obtained, and the melting process can be performed at a high speed with a simple structure. And improve production efficiency.
[Brief description of the drawings]
FIG. 1 is a side view conceptually showing a corrosion-resistant coating forming apparatus used in the method for explaining a corrosion-resistant coating forming method for an inner surface of a cylindrical container according to an embodiment of the present invention.
FIG. 2 is a cross-sectional view showing a cylindrical container obtained by the corrosion-resistant coating forming method according to the embodiment of the present invention.
[Explanation of symbols]
DESCRIPTION OF
Claims (3)