JP3572776B2 - Dielectric material and dielectric film - Google Patents
Dielectric material and dielectric film Download PDFInfo
- Publication number
- JP3572776B2 JP3572776B2 JP02082696A JP2082696A JP3572776B2 JP 3572776 B2 JP3572776 B2 JP 3572776B2 JP 02082696 A JP02082696 A JP 02082696A JP 2082696 A JP2082696 A JP 2082696A JP 3572776 B2 JP3572776 B2 JP 3572776B2
- Authority
- JP
- Japan
- Prior art keywords
- dielectric
- fluorocarbon polymer
- dielectric constant
- film
- dielectric material
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
【0001】
【発明の属する技術分野】
本発明は、半導体装置の形成材料として用いられる誘電体材料および誘電体膜に関し、特に0.25μm以下の設計ルールによるデバイスプロセスに用いられる層間絶縁膜に好適な誘電体材料および誘電率膜に関するものである。
【0002】
【従来の技術】
半導体装置の微細化、低消費電力化および高速化等の要求に伴い、それらを実現するための手段の一つとして層間絶縁膜の低誘電率化が検討されている。
現在開示されている低誘電率材料は、炭素原子やフッ素原子を含有することで誘電率を下げている。現在のところ、誘電率が1.5〜2.5程度のものが実現されている。
【0003】
炭素原子を含む低誘電率材料、すなわち有機系の低誘電率材料としては、有機SOG(Spin on glass)、ポリイミド、ポリパラキシリレンなどが良く知られている。これらの材料は、炭素原子、いわゆるアルキル基を含むことで材料の蜜度が低下すること、および分子自身の分極率が低いことで、低誘電率になっていると言われている。またこれらの材料は、単に誘電率が低いだけでなく、半導体装置の材料として不可欠の耐熱性をも有している。有機SOGはシロキサン構造を持つことで、ポリイミドはイミド結合を持つことで、ポリパラキシリレンはベンゼン環のポリマーとなることで、それぞれ耐熱性を有している。
【0004】
フッ素原子を含む低誘電率材料としては、フッ素を含むシリコン系酸化物(SiOF)が良く知られている。この材料は、シリコン−酸素−シリコン(Si−O−Si)結合をフッ素原子により終端することで材料の密度を下げること、およびフッ素原子自身の分極率の低いこと、などが原因となって誘電率を下げている。当然のことながら、このSiOFは耐熱性にも優れている。
また近年では、従来の半導体装置に用いられているホウ素原子(B)を用いて誘電率を下げるといった検討もなされている。ホウ素原子を含む材料も前述のフッ素原子と同様で、ホウ素自身の分極率が低いこと、ホウ素がSi−O−Si結合のネットワークを短くすること、密度を下げること等が原因となって誘電率を低下させている。
【0005】
さらに最近では、比誘電率が2程度と低いフロロカーボンポリマーが、ULSIデバイスヘ適用できる可能性が高い誘電体材料として注目されている。この材料を用いて半導体装置における誘電体膜を形成する場合には、一旦、フロロカーボンポリマーを溶媒に溶解し、これを下地表面に塗布してから、溶媒を熱処理によって揮発・除去させる工程を行う。
【0006】
【発明が解決しようとする課題】
ところが、従来のフロロカーボンポリマーは、耐熱温度が300℃程度で、無機系の低誘電率材料と比較すると耐熱性が悪く、400℃以上の耐熱温度が要求される半導体装置の形成材料としては不十分である。
また、この材料の耐熱性を向上させる方法として、ハロゲン元素を含む酸などの極性を有する材料を導入して、フロロカーボンポリマーの中に耐熱構造を取り込む方法が知られているが、この方法では誘電率が上がってしまうという不具合が発生する。
【0007】
しかもフロロカーボンポリマーは、ガラス転移温度以上における熱膨張係数がアルミ配線やシリコン酸化膜に比べて非常に大きく、ガラス転移温度以上の温度で大きな体積変化を起こす。このため、例えば図2に示すように、表面にアルミニウム配線22のパターンが形成されたシリコン酸化膜21上に、配線22を覆うようにしてフロロカーボンポリマーの誘電体膜からなる絶縁膜23を形成し、これを熱処理する場合には、次のような問題が生じる。すなわち、ガラス転移温度以上で体積が大きく膨張した絶縁膜23が、温度降下により収縮して配線22のパターン等の微細な凹凸に対応できなくなり、特に0.3μm以下といったような狭い幅のトレンチ内部でボイド24が発生してしまう。そして、ボイド24が発生すると、一般にはその部分の絶縁膜23の絶縁耐圧が劣化してしまい、当然のごとく半導体装置の電気的信頼性が低下すると言われている。なお、図2において配線22のパターンの上下に形成されている膜は、バリアメタル25である。
【0008】
上記の問題を回避するには、熱処理を行わなければよいが、前述したようにフロロカーボン膜の成膜プロセス上、また半導体装置製造プロセス上、それは不可能である。
したがって、耐熱性が向上しかつ熱膨張率が低く抑えられた誘電体材料および誘電体膜の開発が切望されている。
【0009】
【課題を解決するための手段】
請求項1の発明に係る誘電体材料は、環状構造を有するフロロカーボンポリマーに、シラノール基を有するポリマーを混合したものであり、これを上記課題の解決手段とした。
【0010】
請求項2の発明は、半導体装置に形成される誘電体膜であって、環状構造を有するフロロカーボンポリマーに、シラノール基を有するポリマーを混合してなる誘電体材料で形成したものであり、それを上記課題の解決手段とした。
【0011】
請求項1の発明において、フロロカーボンポリマーに混合する樹脂は、結合の強いシラノール基を有しているため、熱振動に対して強く、半導体装置製造プロセスに耐えうる耐熱性を有している。環状構造を有するフロロカーボンポリマーに上記耐熱性の樹脂を混合してなるこの発明の誘電体材料は、シラノール基を有するポリマーが、フロロカーボンポリマーに絡まって該ポリマーを補強するため、熱振動に対して強いものになる。
またシラノール基を有する耐熱性のポリマーも、誘電率が比較的低いものであるため、低誘電率のフロロカーボンポリマーと混合することによる誘電率の上昇が抑制される。
【0012】
請求項2の発明に用いる誘電体材料は、環状構造を有するフロロカーボンポリマーに、補強剤となるシラノール基を有する樹脂を混合してなることから、熱振動に対して強く、かつ混合による誘電率の上昇が抑制された材料となっている。よって、このような誘電体材料で形成された誘電体膜は、フロロカーボンポリマーのみからなる膜よりも耐熱性が向上し、熱処理時の体積変化が抑えられてボイドが発生し難い膜になるとともに、フロロカーボンポリマーの低誘電率をほぼ維持した膜になる。
【0013】
【発明の実施の形態】
以下、本発明に係る誘電体材料および誘電体膜の実施の形態を詳細に説明する。
まず請求項1の発明に係る第1実施形態を説明する。
この実施形態では、環状構造を有するフロロカーボンポリマーとして、下記式〔1〕で 表されるポリテトラフルオロエチレン構造を有するポリマー〔例えばテフロンAF(デュポン製)〕を用いた。
このテフロンAFは、耐熱温度が約350℃であり、誘電率が2.0程度である。
【0014】
【化1】
【0015】
またシラノール基を有する樹脂として、無機SOG〔例えばType2(東京応化製)〕を用いた。そして上記のフロロカーボンポリマーに無機SOGを5重量%混合し、誘電体材料を得た。
無機SOGは、結合の強いシラノール基を有しているため、熱振動に対して強く、半導体装置製造プロセスに耐えうる耐熱性を有している。また誘電率が、〜4.0程度と低いものである。
【0016】
このような耐熱性を有する無機SOGを、環状構造を有するフロロカーボンポリマーに混合すると、フロロカーボンポリマーの鎖に耐熱性の無機SOGの鎖がファンデルワールス力によって絡み合った状態となり、フロロカーボンポリマー構造が補強される。よって上記のごとく調整された誘電体材料は、熱振動に対して強く、耐熱温度が425℃とフロロカーボンポリマーのみと比較して非常に耐熱性が向上したものとなった。またフロロカーボンポリマー構造が補強されるため、熱膨張率が200ppm/℃と低く抑えられたものとなった。さらに混合する無機SOGの誘電率が比較的低いため、混合による誘電率の上昇が抑制され、得られた誘電体材料の誘電率は2.6であった。
【0017】
またこの誘電体材料では、フロロカーボンポリマーと無機SOGとがファンデルワールス力だけで絡み合った状態となっているため、フロロカーボンポリマーに混合する耐熱性の樹脂の割合によって、誘電率、耐熱温度、熱膨張率が直線的に変化する。したがって、フロロカーボンポリマーに対する無機SOGの樹脂の混合割合を変化させるだけで、所望の誘電率、熱膨張率および耐熱温度に調整された誘電体材料を得ることができる。
【0018】
次に請求項1の発明の第2実施形態を説明する。
この実施形態では、シラノール基を有する樹脂として、有機SOG〔例えばHSG(日立化成製)〕を用いた以外は、請求項1の発明に係る第1実施形態と同様にして誘電体材料を得た。
有機SOGも、結合の強いシラノール基を有しているため、熱振動に対して強く、半導体装置製造プロセスに耐えうる耐熱性を有している。また誘電率が、3〜3.5程度と低いものである。
【0019】
このような耐熱性を有する有機SOGを、環状構造を有するフロロカーボンポリマーに混合しても、無機SOGを用いた第1実施形態と同様、フロロカーボンポリマーの鎖に有機SOGの鎖がファンデルワールス力によって絡み合った状態となり、フロロカーボンポリマー構造が補強される。よって上記のごとく調整された誘電体材料は、耐熱温度が420℃とフロロカーボンポリマーのみと比較して非常に耐熱性が向上したものとなった。またフロロカーボンポリマー構造が補強されるため、熱膨張率が200ppm/℃と低く抑えられたものとなった。さらに混合する無機SOGの誘電率が比較的低いことから、混合による誘電率の上昇が抑制され、得られた誘電体材料の誘電率は2.5であった。
【0020】
またこの誘電体材料においても、第1実施形態の場合と同様、フロロカーボンポリマーと有機SOGとがファンデルワールス力だけで絡み合った状態となっているため、フロロカーボンポリマーに混合する耐熱性の樹脂の割合によって、誘電率、耐熱温度、熱膨張率が直線的に変化する。したがって、有機SOGの樹脂の混合割合を変化させるだけで、所望の誘電率、熱膨張率および耐熱温度に調整された誘電体材料を得ることができる。
【0021】
ここで上記実施形態では、フロロカーボンポリマーとしてシクロポリマライズドフロリネーテッドポリマー、ポリテトラフルオロエチレンを用いたが、環状構造を有するものであればよく、これらの例に限定されない。
またフロロカーボンポリマーに混合する樹脂としては、シラノール基を有していればよく、いずれの樹脂を用いることも可能である。例えば下記式〔2〕で表される芳香族ポリアミドを有するものや、ナフタレン環を有するもの、または下記式〔3〕で表されるベンゼン環とともに複素環を有する樹脂などを用いてもよい。
【0022】
【化2】
【0023】
【化3】
【0024】
さらに、環状構造を有するフロロカーボンポリマーとシラノール基を有する樹脂との組み合わせであれば、どのような組み合わせでも上記した実施形態と同様の効果を得ることができる。
【0025】
次に、請求項2の発明に係る誘電体膜の一実施形態を図1に基づいて説明する。なお、ここでは、請求項2の発明を半導体装置における絶縁膜に適用した一例を述べる。
ここではまず、シリコン基板1上に500nm程度の厚さのシリコン酸化膜2を形成する。このシリコン酸化膜2は、一般的なモノシランと酸素とを原料ガスに用いたCVD法で行う。
次いでスパックリング法によって、シリコン酸化膜2に例えばアルミニウム−シリコン合金膜を成膜した後、一般的なレジストプロセスおよびエッチングプロセスにより、上記合金膜をバターニングしてアルミニウム−シリコン合金からなる金属配線3を形成する。
【0026】
次いで、前述した請求項1の発明に係る実施形態の誘電体材料を用い、シリコン酸化膜2上に金属配線3を覆うようにして絶縁膜4を成膜する。成膜装置には、例えば一般的な塗布装置(スピンコーター)を用いることができる。この場合、予め誘電体材料を例えばフロロカーボン系の溶媒(一例としてフロリナート)に溶解し、所定の粘性に調整したものを用いる。
【0027】
例えば誘電体材料を2.0cStに調整し、スピンコーターで成膜する場合には、スピンコートを500rpmの回転数で10秒、3000rpmの回転数で60秒を連続して行う。そして引き続きプレートヒータで150℃にて5分、250℃にて5分間のベーキングを行い、最後に既存の拡散炉を用いて窒素雰囲気中、400℃、30分間のアニールを行う。
【0028】
こうして絶縁膜4を形成した後は、絶縁膜4上にシリコン酸化膜5を例えば10nm程度形成する。この成膜は、温度を350℃、圧力を1kPaとした条件下で、原料ガスにモノシランガスと酸素ガスとを用いて既存のCVD装置で行うことができる。
そしてさらにその上層に、プラズマCVD法によって、シリコン酸化膜6を形成し半導体装置7を得る。シリコン酸化膜6の成膜は、例えば温度を350℃、圧力を30Paとした条件下で、原料ガスにTEOSガスと酸素ガスとを用いて既存の枚葉式プラズマCVD装置で行う。
【0029】
この実施形態によれば、絶縁膜4の形成に、400℃以上の耐熱性を有し、かつ熱膨張率が低く抑えられた誘電体材料を用いているので、熱処理時に分解せず、しかもボイドの発生が抑えられた絶縁膜4を得ることができる。また上記誘電体材料が、フロロカーボンポリマーの誘電率をほぼ維持しているため、絶縁膜4は低誘電率の膜になる。
よって、電気的信頼性が向上しかつ配線3,3間の容量が低減した半導体装置7を製造できるので、半導体装置7に搭載するデバイスの動作の高速化を図ることができる。
【0030】
【発明の効果】
以上鋭明したように請求項1記載の発明の誘電体材料では、環状構造を有するフロロカーボンポリマーに、補強剤となるシラノール基を有する耐熱性の樹脂が混合されており、また、フロロカーボンポリマーと上記耐熱性の樹脂とを混合することによる誘電率の上昇が抑制されるので、フロロカーボンポリマーの低誘電率の維持が可能になる。よって、半導体装置の誘電体膜の形成材料として非常に好適なものになる。
【0031】
請求項2の発明の誘電体膜では、環状構造を有するフロロカーボンポリマーに、補強剤となるシラノール基を有する耐熱性の樹脂を混合されて、耐熱性が向上し、熱膨張率が抑制され、混合による誘電率の上昇が抑制された誘電体材料を用いているので、熱処理時の分解およびボイドの発生を防止でき、かつフロロカーボンの低誘電率をほぼ維持することができる。よって、半導体装置の誘電体膜として使用すれば、電気的信頼性が向上しかつ配線間の容量が低減した半導体装置を製造できるので、半導体装置に搭載するデバイスの動作の高速化を図ることができる。
【図面の簡単な説明】
【図1】本発明の誘電体膜の形成例を示す概略断面図である。
【図2】本発明の課題を説明するための概略断面図である。
【符号の説明】
4 絶縁膜(誘電体膜)[0001]
TECHNICAL FIELD OF THE INVENTION
The present invention relates to a dielectric material and the dielectric film is used as a material for forming a semiconductor device, relates to a suitable dielectric material and dielectric constant film on the interlayer insulating film used in the device process due particularly 0.25μm following design rules Things.
[0002]
[Prior art]
With demands for miniaturization, low power consumption, high speed, and the like of semiconductor devices, lowering the dielectric constant of an interlayer insulating film is being studied as one of means for realizing them.
Currently disclosed low dielectric constant materials lower the dielectric constant by containing carbon atoms and fluorine atoms. At present, those having a dielectric constant of about 1.5 to 2.5 have been realized.
[0003]
As a low dielectric constant material containing a carbon atom, that is, an organic low dielectric constant material, organic SOG (Spin on glass), polyimide, polyparaxylylene, and the like are well known. It is said that these materials have a low dielectric constant due to a decrease in the nectarity of the material by including a carbon atom, a so-called alkyl group, and a low polarizability of the molecule itself. These materials not only have a low dielectric constant but also have heat resistance indispensable as a material for a semiconductor device. The organic SOG has a siloxane structure, the polyimide has an imide bond, and the polyparaxylylene becomes a benzene ring polymer, and thus has heat resistance.
[0004]
As a low dielectric constant material containing a fluorine atom, a silicon-based oxide (SiOF) containing fluorine is well known. This material has a dielectric loss due to a decrease in the density of the material by terminating a silicon-oxygen-silicon (Si-O-Si) bond with a fluorine atom, and a low polarizability of the fluorine atom itself. The rate is decreasing. As a matter of course, this SiOF is also excellent in heat resistance.
In recent years, studies have been made to lower the dielectric constant using boron atoms (B) used in conventional semiconductor devices. The material containing a boron atom is also similar to the above-mentioned fluorine atom, and has a low dielectric constant due to the low polarizability of boron itself, the shortening of the network of the Si-O-Si bond by boron, and the reduction of the density. Is decreasing.
[0005]
More recently, fluorocarbon polymers having a relative dielectric constant as low as about 2 have attracted attention as a dielectric material having a high possibility of being applicable to ULSI devices. When a dielectric film in a semiconductor device is formed using this material, a process of once dissolving a fluorocarbon polymer in a solvent, applying the solution on a base surface, and then volatilizing and removing the solvent by heat treatment is performed.
[0006]
[Problems to be solved by the invention]
However, the conventional fluorocarbon polymer has a heat resistance temperature of about 300 ° C., and has poor heat resistance as compared with inorganic low dielectric constant materials, and is insufficient as a material for forming a semiconductor device requiring a heat resistance temperature of 400 ° C. or higher. It is.
As a method for improving the heat resistance of this material, a method of introducing a heat-resistant structure into a fluorocarbon polymer by introducing a polar material such as an acid containing a halogen element is known. There is a problem that the rate increases.
[0007]
In addition, the fluorocarbon polymer has a very large coefficient of thermal expansion above the glass transition temperature as compared with aluminum wiring or a silicon oxide film, and causes a large volume change at a temperature above the glass transition temperature. For this reason, as shown in FIG. 2 , for example, an
[0008]
In order to avoid the above problem, heat treatment is not required. However, as described above, it is impossible in the process of forming a fluorocarbon film and in the process of manufacturing a semiconductor device.
Therefore, development of a dielectric material and a dielectric film having improved heat resistance and a low coefficient of thermal expansion has been desired.
[0009]
[Means for Solving the Problems]
The dielectric material according to the first aspect of the present invention is obtained by mixing a fluorocarbon polymer having a cyclic structure with a polymer having a silanol group .
[00 10 ]
According to a second aspect of the present invention, there is provided a dielectric film formed on a semiconductor device, wherein the dielectric film is formed of a dielectric material obtained by mixing a polymer having a silanol group with a fluorocarbon polymer having a cyclic structure. This is means for solving the above problems.
[00 11]
According to the first aspect of the present invention, since the resin mixed with the fluorocarbon polymer has a silanol group having a strong bond, the resin is resistant to thermal vibration and has heat resistance enough to withstand a semiconductor device manufacturing process. The dielectric material of the present invention, which is obtained by mixing the above-mentioned heat-resistant resin with a fluorocarbon polymer having a cyclic structure, the polymer having a silanol group is entangled with the fluorocarbon polymer to reinforce the polymer. Become something.
Also, since the heat-resistant polymer having a silanol group has a relatively low dielectric constant, an increase in the dielectric constant caused by mixing with a fluorocarbon polymer having a low dielectric constant is suppressed.
[00 12 ]
Since the dielectric material used in the invention of
[00 13 ]
BEST MODE FOR CARRYING OUT THE INVENTION
Hereinafter, embodiments of the dielectric material and the dielectric film according to the present invention will be described in detail.
First, a first embodiment according to the first aspect of the present invention will be described.
In this embodiment , a polymer having a polytetrafluoroethylene structure represented by the following formula [1] [for example, Teflon AF (manufactured by DuPont)] was used as the fluorocarbon polymer having a cyclic structure.
This Teflon AF has a heat resistant temperature of about 350 ° C. and a dielectric constant of about 2.0.
[00 14 ]
Embedded image
[00 15 ]
As the resin having a silanol group, an inorganic SOG [for example, Type 2 (manufactured by Tokyo Ohka)] was used. Then, 5% by weight of inorganic SOG was mixed with the above fluorocarbon polymer to obtain a dielectric material.
Since the inorganic SOG has a strong bond silanol group, it is resistant to thermal vibration and has heat resistance that can withstand the semiconductor device manufacturing process. Further, the dielectric constant is as low as about 4.0.
[00 16]
When such heat-resistant inorganic SOG is mixed with a fluorocarbon polymer having a cyclic structure, the heat-resistant inorganic SOG chain is entangled with the fluorocarbon polymer chain by Van der Waals force, and the fluorocarbon polymer structure is reinforced. You. Therefore, the dielectric material adjusted as described above is resistant to thermal vibration, has a heat resistance temperature of 425 ° C., and has significantly improved heat resistance as compared with the fluorocarbon polymer alone. Further, since the fluorocarbon polymer structure was reinforced, the coefficient of thermal expansion was suppressed to as low as 200 ppm / ° C. Further, since the dielectric constant of the mixed inorganic SOG was relatively low, the increase in the dielectric constant due to the mixing was suppressed, and the dielectric constant of the obtained dielectric material was 2.6.
[00 17]
Further, in this dielectric material, since the fluorocarbon polymer and the inorganic SOG are intertwined only by van der Waals force, the dielectric constant, the heat resistance temperature, and the thermal expansion are determined by the ratio of the heat-resistant resin mixed with the fluorocarbon polymer. The rate changes linearly. Therefore, only by changing the mixing ratio of the inorganic SOG resin to the fluorocarbon polymer, it is possible to obtain a dielectric material adjusted to a desired dielectric constant, thermal expansion coefficient and heat-resistant temperature.
[00 18 ]
Next will be described a second embodiment of the invention of
In this embodiment, as the resin having a silanol group, except for using an organic SOG [e.g. HSG (Hitachi Chemical Co., Ltd.)], to obtain a dielectric material in the same manner as in the first embodiment according to the invention of
Since organic SOG also has a strong bond silanol group, it is resistant to thermal vibration and has heat resistance that can withstand the semiconductor device manufacturing process. Further, the dielectric constant is as low as about 3 to 3.5.
[00 19 ]
Even when the organic SOG having such heat resistance is mixed with the fluorocarbon polymer having a cyclic structure, the organic SOG chains are added to the fluorocarbon polymer chains by van der Waals force as in the first embodiment using the inorganic SOG. It becomes entangled and reinforces the fluorocarbon polymer structure. Therefore, the dielectric material adjusted as described above has a heat resistance temperature of 420 ° C., which is much higher in heat resistance than fluorocarbon polymer alone. Further, since the fluorocarbon polymer structure was reinforced, the coefficient of thermal expansion was suppressed to as low as 200 ppm / ° C. Further, since the dielectric constant of the mixed inorganic SOG was relatively low, the increase in the dielectric constant due to the mixing was suppressed, and the dielectric constant of the obtained dielectric material was 2.5.
[00 20 ]
Also in this dielectric material, since the fluorocarbon polymer and the organic SOG are intertwined only by Van der Waals force, as in the case of the first embodiment, the ratio of the heat-resistant resin mixed with the fluorocarbon polymer is Accordingly, the dielectric constant, the allowable temperature limit, and the coefficient of thermal expansion linearly change. Therefore, only by changing the mixing ratio of the organic SOG resin, a dielectric material adjusted to a desired dielectric constant, thermal expansion coefficient, and heat-resistant temperature can be obtained.
[00 21 ]
Here, in the above-described embodiment, the cyclopolymerized fluorinated polymer and polytetrafluoroethylene are used as the fluorocarbon polymer. However, the present invention is not limited to these examples as long as it has a cyclic structure.
As the resin to be mixed with the fluorocarbon polymer, any resin may be used as long as it has a silanol group, and any resin can be used. For example, a resin having an aromatic polyamide represented by the following formula [2], a resin having a naphthalene ring, or a resin having a heterocyclic ring together with a benzene ring represented by the following formula [3] may be used.
[00 22 ]
Embedded image
[00 23 ]
Embedded image
[00 24 ]
Further, any combination of a fluorocarbon polymer having a cyclic structure and a resin having a silanol group can provide the same effects as those of the above-described embodiment.
[00 25]
Next, an embodiment of the dielectric film according to the second aspect of the present invention will be described with reference to FIG . Here, an example in which the invention of
Here, first, a
Next, for example, an aluminum-silicon alloy film is formed on the
[00 26]
Then, a dielectric material of embodiments according to the invention of
[00 27]
For example, when a dielectric material is adjusted to 2.0 cSt and a film is formed by a spin coater, spin coating is continuously performed at a rotation speed of 500 rpm for 10 seconds and at a rotation speed of 3000 rpm for 60 seconds. Subsequently, baking is performed at 150 ° C. for 5 minutes and at 250 ° C. for 5 minutes using a plate heater, and finally annealing is performed at 400 ° C. for 30 minutes in a nitrogen atmosphere using an existing diffusion furnace .
[00 28 ]
After the formation of the insulating film 4, a silicon oxide film 5 is formed on the insulating film 4, for example, with a thickness of about 10 nm. This film formation can be performed by an existing CVD apparatus under the conditions of a temperature of 350 ° C. and a pressure of 1 kPa, using a monosilane gas and an oxygen gas as a source gas.
Then, a
[00 29 ]
According to this embodiment, the insulating film 4 is formed of a dielectric material having heat resistance of 400 ° C. or higher and having a low coefficient of thermal expansion. Can be obtained. Since the dielectric material substantially maintains the dielectric constant of the fluorocarbon polymer, the insulating film 4 has a low dielectric constant.
Therefore, the semiconductor device 7 with improved electrical reliability and reduced capacitance between the
[00 30 ]
【The invention's effect】
The dielectric material of the first aspect as SurudoAkira above, the fluorocarbon polymer having a cyclic structure, heat-resistant resin having a silanol group as a reinforcing agent are mixed, also fluorocarbon polymer and the Since an increase in the dielectric constant caused by mixing with a heat-resistant resin is suppressed, the low dielectric constant of the fluorocarbon polymer can be maintained. Therefore, it is very suitable as a material for forming a dielectric film of a semiconductor device.
[00 31 ]
In the dielectric film according to the second aspect of the present invention, a fluorocarbon polymer having a cyclic structure is mixed with a heat-resistant resin having a silanol group as a reinforcing agent, thereby improving heat resistance and suppressing a coefficient of thermal expansion. Since the dielectric material whose rise in the dielectric constant is suppressed is used, decomposition and generation of voids during the heat treatment can be prevented, and the low dielectric constant of the fluorocarbon can be almost maintained. Therefore, when used as a dielectric film of a semiconductor device , a semiconductor device with improved electrical reliability and reduced capacitance between wirings can be manufactured, so that the speed of operation of a device mounted on the semiconductor device can be increased. it can.
[Brief description of the drawings]
FIG. 1 is a schematic sectional view showing an example of forming a dielectric film of the present invention.
FIG. 2 is a schematic sectional view for explaining a problem of the present invention.
[Explanation of symbols]
4 Insulating film (dielectric film)
Claims (2)
ことを特徴とする誘電体材料。A dielectric material comprising a fluorocarbon polymer having a cyclic structure and a polymer having a silanol group mixed therein.
環状構造を有するフロロカーボンポリマーに、シラノール基を有するポリマーが混合されてなる誘電体材料で形成されている
ことを特徴とする誘電体膜。A dielectric film formed on a semiconductor device,
1. A dielectric film comprising a dielectric material obtained by mixing a fluorocarbon polymer having a cyclic structure with a polymer having a silanol group.