JP3400281B2 - Leather-like sheet and method for producing the same - Google Patents
Leather-like sheet and method for producing the sameInfo
- Publication number
- JP3400281B2 JP3400281B2 JP03011997A JP3011997A JP3400281B2 JP 3400281 B2 JP3400281 B2 JP 3400281B2 JP 03011997 A JP03011997 A JP 03011997A JP 3011997 A JP3011997 A JP 3011997A JP 3400281 B2 JP3400281 B2 JP 3400281B2
- Authority
- JP
- Japan
- Prior art keywords
- polyurethane
- parts
- layer
- resin
- sheet
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
【0001】[0001]
【発明の属する技術分野】本発明は、表面の耐擦過傷
性、耐摩耗性、耐屈曲性および滑り性に優れた皮革様シ
ートおよびその製造方法に関するものである。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a leather-like sheet having excellent surface abrasion resistance, abrasion resistance, bending resistance and slippage, and a method for producing the same.
【0002】[0002]
【従来の技術】従来、表面強度の高い皮革様シートに関
しては様々なものが提供されている。例えば基体層上
に、最表面がブリネル硬さが20〜100である微粒子
を含有するポリウレタンであるコート層を形成した皮革
様シートが知られている。また基体層上に、最表面が1
00%モジュラス100kg/cm2以上の1液型ウレ
タンであるコート層を形成した皮革様シート、あるいは
基体層上に、シリコン変性ウレタン層を表面層とするコ
ート層を形成させ、表面を滑らせることによって耐傷性
を向上させた皮革様シートも知られている。2. Description of the Related Art Conventionally, various leather-like sheets having high surface strength have been provided. For example, a leather-like sheet is known in which a coat layer made of polyurethane containing fine particles having a Brinell hardness of 20 to 100 is formed on the outermost surface of a base layer. The outermost surface is 1 on the base layer.
To form a coat layer having a silicone-modified urethane layer as a surface layer on a leather-like sheet having a coat layer formed of a one-component urethane having a 00% modulus of 100 kg / cm 2 or more, or a base layer, and sliding the surface. A leather-like sheet having improved scratch resistance is also known.
【0003】[0003]
【発明が解決しようとする課題】しかしながら、従来よ
り提案されている方法のうち、ブリネル硬さ20〜10
0の微粒子を含有するポリウレタンの場合においては、
ツヤ感に悪影響を及ぼしやすく、耐傷性に関しては表面
に露出した場合、傷の促進に繋がるという欠点があっ
た。また100%モジュラスにおいて100kg/cm
2以上の1液型ウレタン層を形成した皮革様シートにお
いては、耐傷性はかなり向上するものの、瞬間的な擦過
傷に対してはほとんど効果が認められなかった。同様に
コート層の最表面をシリコン変性ウレタン層としたもの
においても瞬間的な擦過傷に対してほとんど効果がなく
有効な手段とはなり得ない。本発明は、最表面の耐擦過
傷性、耐摩耗性、耐屈曲性および、滑り性に優れた皮革
様シートおよびその製造方法を提供するものである。However, among the methods conventionally proposed, the Brinell hardness of 20 to 10 is used.
In the case of a polyurethane containing 0 fine particles,
It has a drawback that it tends to have an adverse effect on the glossiness, and in terms of scratch resistance, when exposed to the surface, it promotes scratches. 100 kg / cm at 100% modulus
In the leather-like sheet having two or more one-pack type urethane layers formed, scratch resistance was considerably improved, but almost no effect was recognized against instantaneous scratches. Similarly, even if the outermost surface of the coat layer is a silicone-modified urethane layer, it is hardly effective against instantaneous scratches and cannot be an effective means. The present invention provides a leather-like sheet having excellent scratch resistance, abrasion resistance, bending resistance and slipperiness on the outermost surface, and a method for producing the same.
【0004】[0004]
【課題を解決するための手段】本発明者らは、表面を構
成する樹脂組成と乾式造面用離型紙に着目し、鋭意検討
を行った結果、繊維集合体に弾性重合体を主体とした重
合体を含有した基体層(A)の表面に、数平均分子量が
2万〜10万の2液型ポリウレタン樹脂(a)と数平均
分子量が13万〜28万の2液型ポリウレタン樹脂
(b)および該樹脂(a)と(b)の合計重量に対して
固形分比で10〜75重量%のポリイソシアネート硬化
剤を含むポリウレタン樹脂層を最表面に設けることによ
り表面の耐傷性、耐擦過傷性、耐摩耗性、耐屈曲性およ
び滑り性が大きく改善されることを見いだし本発明を完
成するに至った。さらに離型性を向上させるために、最
表面コーテイング層をポリオレフィン系にした離型紙上
に該混合樹脂溶液を塗布することによって、今まで離型
紙と2液型ポリウレタン層が剥がれずに離型性不良を起
こしていたことを改善することが可能となることを見い
だし本発明を完成するに至った。Means for Solving the Problems The present inventors have paid attention to the resin composition constituting the surface and the release paper for dry surface-making, and as a result of diligent study, as a result, the fiber assembly was mainly composed of an elastic polymer. On the surface of the base layer (A) containing a polymer, a two-component polyurethane resin (a) having a number average molecular weight of 20,000 to 100,000 and a two-component polyurethane resin (b) having a number average molecular weight of 130,000 to 280,000. ) And a polyurethane resin layer containing a polyisocyanate curing agent in a solid content ratio of 10 to 75% by weight with respect to the total weight of the resins (a) and (b) is provided on the outermost surface, the surface has scratch resistance and scratch resistance. The inventors have found that the properties, abrasion resistance, flex resistance and slippage are greatly improved, and have completed the present invention. In order to further improve the releasability, by coating the mixed resin solution on a release paper whose outermost surface coating layer is made of polyolefin, the release paper and the two-component polyurethane layer have not been peeled until now. The inventors have found that it is possible to improve the fact that a defect has occurred, and have completed the present invention.
【0005】すなわち本発明の皮革様シートは、繊維集
合体に弾性重合体を主体とした重合体を含有した基体層
(A)上に、ポリウレタン樹脂を主体とする樹脂からな
る接着剤層(B)を介して、数平均分子量が2万〜10
万の2液型ポリウレタン樹脂(a)と数平均分子量が1
3万〜28万の2液型ポリウレタン樹脂(b)が、ポリ
イソシアネート系硬化剤により架橋された樹脂からなる
層(C)が積層されており、さらには、ポリウレタン
(a)とポリウレタン(b)のブレンド重量比が0.0
5〜4であることを特徴とするものである。That is, the leather-like sheet of the present invention comprises a base layer (A) containing a polymer mainly composed of an elastic polymer in a fiber assembly, and an adhesive layer (B composed of a resin mainly composed of polyurethane resin) on the base layer (A). ), The number average molecular weight is 20,000 to 10
Tens of two-component polyurethane resin (a) and number average molecular weight of 1
30,000 to 280,000 two-component polyurethane resin (b) is laminated with a layer (C) made of a resin cross-linked by a polyisocyanate curing agent, and further, polyurethane (a) and polyurethane (b) Blend weight ratio of 0.0
It is characterized by being 5 to 4.
【0006】また本発明の皮革様シートの製造方法は、
数平均分子量が2万〜10万の2液型ポリウレタン樹脂
(a)と数平均分子量が13万〜28万の2液型ポリウ
レタン樹脂(b)および該樹脂(a)と(b)の合計重
量に対して固形分比10〜75重量%のポリイソシアネ
ート硬化剤を含むポリウレタン樹脂を離型紙上に塗布
し、乾燥して層(C)を形成した後、接着層(B)を介
して、繊維集合体に弾性重合体を主体とした重合体を含
有した基体層に貼着し硬化反応を行わせた後、該離型紙
を剥離することを特徴とするものである。The method for producing a leather-like sheet of the present invention is
Two-component polyurethane resin (a) having a number average molecular weight of 20,000 to 100,000, two-component polyurethane resin (b) having a number average molecular weight of 130,000 to 280,000, and the total weight of the resins (a) and (b). A polyurethane resin containing a polyisocyanate curing agent having a solid content ratio of 10 to 75% by weight is coated on a release paper and dried to form a layer (C), and then a fiber is formed through an adhesive layer (B). The release paper is peeled off after the assembly is adhered to a base layer containing a polymer mainly composed of an elastic polymer to cause a curing reaction.
【0007】以下本発明について詳述する。本発明の皮
革様シートの基体層(A)は、繊維集合体に弾性重合体
を主体とした重合体を含有したシートである。The present invention will be described in detail below. The base layer (A) of the leather-like sheet of the present invention is a sheet containing a polymer mainly composed of an elastic polymer in a fiber assembly.
【0008】本発明の基体層(A)の製造に用いられる
繊維集合体は、通常の繊維、例えば、ポリエステル、ポ
リアミド、ポリアクリロニトリル、ポリオレフィン、ポ
リビニルアルコールなどの合成繊維、再生セルロースな
どの化学繊維、天然繊維、又は特殊形態の繊維、例えば
ポリエステル、ポリアミド、ポリアクリロニトリル等の
極細繊維、あるいは少なくとも2種類のポリマーからな
る極細繊維発生型繊維からつくられる。例えば、海成分
が溶剤または水酸化ナトリウム等の分解剤により溶解ま
たは分解することで島成分にフィブリル化するような断
面である海島構造を有する抽出型又は分解型繊維、ある
いは機械的にまたは処理剤によってポリマーの界面で剥
離が生じて各ポリマーからなる極細繊維にフィブリル化
する分割型繊維等があげられる。The fiber assembly used in the production of the base layer (A) of the present invention includes ordinary fibers such as synthetic fibers such as polyester, polyamide, polyacrylonitrile, polyolefin and polyvinyl alcohol, and chemical fibers such as regenerated cellulose. It is made of natural fibers or fibers of a special form, for example, ultrafine fibers such as polyester, polyamide, polyacrylonitrile, etc., or ultrafine fiber generating fibers composed of at least two kinds of polymers. For example, an extractable or degradable fiber having a sea-island structure having a cross section such that the sea component is dissolved or decomposed by a solvent or a decomposing agent such as sodium hydroxide into an island component, or mechanically or a treating agent. As a result, there is a split-type fiber or the like in which separation occurs at the polymer interface and fibrillates into ultrafine fibers made of each polymer.
【0009】極細繊維を構成するポリマーとしては、6
−ナイロン、66−ナイロンをはじめとする溶融紡糸可
能なポリアミド類、ポリエチレンテレフタレート、ポリ
ブチレンテレフタレート、カチオン可染型変性ポリエチ
レンテレフタレートをはじめとする溶融紡糸可能なポリ
エステル類、ポリプロピレンで代表されるポリオレフィ
ン類などから選ばれた少なくとも1種類のポリマーが挙
げられる。また、抽出型又は分解型繊維で抽出または分
解除去される成分としては、極細繊維成分とは溶剤また
は分解剤に対する溶解性または分解性を異にし、極細繊
維成分との相溶性の小さいポリマーであり、かつ紡糸条
件下で極細繊維成分より溶融粘度が小さいかあるいは表
面張力が小さいポリマーであり、例えば、ポリエチレ
ン、ポリスチレン、ポリエチレンプロピレン共重合体、
変性ポリエステルなどのポリマーから選ばれた少なくと
も1種類のポリマーである。As the polymer constituting the ultrafine fibers, 6
-Nylon, melt-spinnable polyamides such as 66-nylon, polyethylene terephthalate, polybutylene terephthalate, melt-spinnable polyesters such as cationic dyeable modified polyethylene terephthalate, polyolefins represented by polypropylene, etc. At least one polymer selected from Further, the component extracted or decomposed and removed by the extractable or degradable fiber is a polymer having a different solubility or degradability in a solvent or a degrading agent from the ultrafine fiber component and having a small compatibility with the ultrafine fiber component. , And a polymer having a smaller melt viscosity or a smaller surface tension than the ultrafine fiber component under spinning conditions, for example, polyethylene, polystyrene, polyethylene propylene copolymer,
It is at least one polymer selected from polymers such as modified polyester.
【0010】この極細繊維の海成分と島成分の重量比は
1:2〜2:1であって、海成分を抽出した後の島成分
の好適デニールとしては風合いや充実感の点で、0.0
1〜0.0001デニールの範囲が好ましい。これらの
繊維をウェッブとし、ニードルパンチや高速流体流によ
り絡合して不織布とする。不織布の目付は300〜15
00g/m2が好ましく、より好ましくは500〜10
00g/m2であり、300g/m2未満の場合には繊維
量の不足によりゴムライクとなり、1500g/m2を
超える場合には柔軟性のない皮革様シートとなる。さら
に厚みは0.8〜4mmが好ましく、より好ましくは1
〜3mmであり、0.8mm未満あるいは4mmを越え
る厚みの場合には、造面した時のバランスが悪く、ゴム
ライクあるいは柔軟性のないものとなる。The weight ratio of the sea component to the island component of this ultrafine fiber is 1: 2 to 2: 1. As a preferable denier of the island component after extracting the sea component, in terms of texture and fullness, 0 .0
A range of 1 to 0.0001 denier is preferred. These fibers are used as webs and entangled by needle punching or high-speed fluid flow to form a nonwoven fabric. Nonwoven fabric weight is 300 to 15
00 g / m 2 is preferable, and more preferably 500 to 10
Was 00g / m 2, becomes rubber-like due to insufficient amount fiber in the case of less than 300 g / m 2, the inflexible leather-like sheet in the case of more than 1500 g / m 2. Further, the thickness is preferably 0.8 to 4 mm, more preferably 1
When the thickness is less than 0.8 mm or more than 4 mm, the balance at the time of making a surface is poor, and it becomes rubber-like or inflexible.
【0011】次に繊維絡合不織布に弾性樹脂液を含浸
し、加熱乾燥することでゲル化させるかあるいは弾性樹
脂の非溶剤を含む液に浸漬して湿式凝固することで緻密
な発泡スポンジを形成する。ここで含浸する弾性樹脂と
しては、例えば平均分子量500〜3000のポリエス
テルジオール、ポリエーテルジオール、ポリカーボネー
トジオールあるいはポリエステルポリエーテルジオール
等の複合ジオール等から選ばれた少なくとも1種類のポ
リマージオールと、4,4’−ジフェニルメタンジイソ
シアネート(MDI)、イソホロンジイソシアネート
(IPDI)、ヘキサメチレンジイソシアネート(HD
I)などの芳香族系、脂環族系、脂肪族系のジイソシア
ネートなどから選ばれた少なくとも1種類のジイソシア
ネートと、2個以上の活性水素原子を有する少なくとも
1種類の低分子化合物で分子量300以下の化合物、例
えば、エチレングリコール、プロピレングリコール、
1.4ーブタンジオール、ヘキサンジオール、3−メチ
ル−1,5−ペンタンジオール、1,4−シクロヘキサ
ンジオール、キシレングリコール等のジオール類、エチ
レンジアミン、プロピレンジアミン、キシリレンジアミ
ン、イソホロンジアミン、ピペラジン、フェニレンジア
ミン、トリレンジアミン等のジアミン類、アジピン酸ヒ
ドラジド、イソフタル酸ジヒドラジド等のヒドラジン或
いはヒドラジド類等から選ばれた少なくとも1種類とを
反応させて得たポリウレタンである。特に好ましくは、
1,4−ブタンジオールまたは3−メチル−1,5−ペ
ンタンジオールを主体とした鎖伸長剤を所定のモル比で
反応させて得たポリウレタンおよびその変性物である。Next, the fiber-entangled non-woven fabric is impregnated with an elastic resin liquid and gelled by heating and drying, or by immersing in a liquid containing a non-solvent of the elastic resin and wet coagulation to form a dense foam sponge. To do. Examples of the elastic resin impregnated here include at least one polymer diol selected from composite diols having an average molecular weight of 500 to 3000, such as polyester diol, polyether diol, polycarbonate diol, polyester polyether diol, and the like; '-Diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HD
I) such as at least one kind of diisocyanate selected from aromatic, alicyclic and aliphatic diisocyanates and at least one kind of low molecular weight compound having two or more active hydrogen atoms and having a molecular weight of 300 or less. A compound of, for example, ethylene glycol, propylene glycol,
1.4-butanediol, hexanediol, 3-methyl-1,5-pentanediol, 1,4-cyclohexanediol, diols such as xylene glycol, ethylenediamine, propylenediamine, xylylenediamine, isophoronediamine, piperazine, phenylenediamine, A polyurethane obtained by reacting with at least one selected from diamines such as tolylenediamine, hydrazine such as adipic acid hydrazide and isophthalic acid dihydrazide, hydrazides and the like. Particularly preferably,
A polyurethane obtained by reacting a chain extender mainly composed of 1,4-butanediol or 3-methyl-1,5-pentanediol at a predetermined molar ratio and a modified product thereof.
【0012】またポリエステルエラストマー等の他の弾
性樹脂およびアクリル系等の弾性樹脂であってもよい。
またこれらを混合した重合体組成物でもよい。しかし、
柔軟性、弾性回復性、スポンジ形成性等より上記のポリ
ウレタンが好ましく用いられる。なお不織布に含浸する
際の弾性体のポリマー濃度は10〜50%が好ましく、
ヤング率は1〜15kg/mm2の範囲が好ましい。ま
た上記ポリウレタンとしてポリマージオールと上記低分
子化合物のモル比が1:1〜1:7の範囲であるポリウ
レタンが好ましい。このポリウレタンを溶媒で溶解ある
いは希釈して繊維絡合不織布に含浸する。ここで使用す
る溶媒はジメチルスルホキシド、スルホラン、ジメチル
ホルムアミド、ジメチルアセトアミド、Nーメチルピロ
リドン、ジフェニルスルホン、N,N’−ジメチルイミ
ダゾリノン等であり、特にジメチルホルムアミドが好適
に用いられる。また溶解あるいは希釈したポリウレタン
液中のポリウレタン濃度は5〜30重量%が好ましく、
特に好ましくは10〜20重量%である。Further, other elastic resin such as polyester elastomer and elastic resin such as acrylic resin may be used.
A polymer composition obtained by mixing these may also be used. But,
The above-mentioned polyurethane is preferably used because of its flexibility, elastic recovery property, sponge forming property and the like. The polymer concentration of the elastic body when impregnating the nonwoven fabric is preferably 10 to 50%,
The Young's modulus is preferably in the range of 1 to 15 kg / mm 2 . Further, as the polyurethane, a polyurethane in which the molar ratio of the polymer diol and the low molecular weight compound is in the range of 1: 1 to 1: 7 is preferable. This polyurethane is dissolved or diluted with a solvent to impregnate the fiber-entangled nonwoven fabric. The solvent used here is dimethyl sulfoxide, sulfolane, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, diphenylsulfone, N, N'-dimethylimidazolinone, etc., and dimethylformamide is particularly preferably used. The concentration of polyurethane in the dissolved or diluted polyurethane liquid is preferably 5 to 30% by weight,
It is particularly preferably 10 to 20% by weight.
【0013】含浸したポリウレタン液はポリウレタンの
非溶剤中で凝固、脱洗させるか、あるいは乾式法により
ゲル化凝固させた後、パークレンやトリクレンやトルエ
ン等の液中に浸漬することにより多成分繊維(極細繊維
発生型繊維)を極細繊維束状繊維にすることで基体層を
作製する。なお極細化と弾性重合体の含浸は順序を逆に
してもよい。基体層の厚みは得られた皮革様シートの用
途により任意に選択でき、特に限定されるものではない
が、造面層とのバランスの点から好ましくは0.5〜3
mmであり、より好ましくは0.5〜2mmの範囲であ
る。また基体層の比重は好ましくは0.2〜0.7g/
cm3であり、より好ましくは0.3〜0.5g/cm3
の範囲である。基体層を構成する繊維と弾性重合体との
重量比は90:10〜40:60の範囲が好ましい。The impregnated polyurethane liquid is coagulated and dewashed in a non-solvent of polyurethane, or after gelling and coagulation by a dry method, it is immersed in a liquid such as Perkren, trichlene, toluene or the like to prepare multi-component fibers ( The base layer is prepared by forming (ultrafine fiber-generating fiber) into a bundle of ultrafine fibers. Note that the order of ultrafine and impregnation with the elastic polymer may be reversed. The thickness of the base layer can be arbitrarily selected depending on the intended use of the obtained leather-like sheet and is not particularly limited, but is preferably 0.5 to 3 from the viewpoint of balance with the surface layer.
mm, and more preferably 0.5 to 2 mm. The specific gravity of the base layer is preferably 0.2 to 0.7 g /
cm 3 , and more preferably 0.3 to 0.5 g / cm 3.
Is the range. The weight ratio of the fibers constituting the base layer and the elastic polymer is preferably 90:10 to 40:60.
【0014】本発明において、表面層(C)を構成する
架橋型弾性重合体樹脂を構成するポリウレタンの種類は
特に限定されず、例えばポリエステル系、ポリエーテル
系、ポリカーボネート系あるいはそれらのブレンドまた
はその変性体等が挙げられるが、耐久性や物性等を考慮
するとポリエーテル系またはポリカーボネート系が好ま
しい。In the present invention, the type of polyurethane constituting the crosslinked elastic polymer resin constituting the surface layer (C) is not particularly limited, and examples thereof include polyester type, polyether type, polycarbonate type, blends thereof or modifications thereof. Examples thereof include a body, and in consideration of durability and physical properties, a polyether type or a polycarbonate type is preferable.
【0015】表面層(C)を構成する樹脂は、数平均分
子量が2万〜10万の2液型ポリウレタン樹脂(a)と
数平均分子量が13万〜28万の2液型ポリウレタン樹
脂(b)のブレンド物の架橋物であり、ポリウレタン
(a)とポリウレタン(b)のブレンド重量比率(a)
/(b)は0.05〜4が好ましく、0.05未満の場
合には耐擦過傷性、耐摩耗性および滑り性は良いが耐屈
曲性が悪い欠点がある。(a)/(b)が4を越える場
合には最表面のタックが有りすぎて滑り性が悪くなる。
また表面粘着性が大きいためブロッキングが発生すると
いった欠点がある。The resin constituting the surface layer (C) includes a two-component polyurethane resin (a) having a number average molecular weight of 20,000 to 100,000 and a two-component polyurethane resin (b) having a number average molecular weight of 130,000 to 280,000. ), Which is a cross-linked product of the blended product of (a) and polyurethane (a) and polyurethane (b).
/ (B) is preferably from 0.05 to 4, and when it is less than 0.05, there is a defect that abrasion resistance, abrasion resistance and slidability are good, but bending resistance is bad. When (a) / (b) exceeds 4, tackiness on the outermost surface is excessive and slipperiness deteriorates.
In addition, there is a drawback that blocking occurs due to high surface tackiness.
【0016】さらに数平均分子量が10万よりも小さい
ポリウレタン樹脂単品で使用すると造面後のタックがか
なりあるため縫製その他の工程通過性に問題があり、数
平均分子量13万以上のポリウレタン樹脂単品で使用す
ると造面後のタックは良好であるが、耐擦過傷性、耐屈
曲性が落ちるといった問題がある。また、数平均分子量
10万〜13万のポリウレタン樹脂単品で使用すると耐
擦過傷性が十分でなく、かつタックが出てくるため縫製
その他の工程通過性に問題がある。Further, when used as a single polyurethane resin having a number average molecular weight of less than 100,000, there is a problem in passingability in sewing and other processes because there is considerable tack after the surface is made. When used, the tack after fabrication is good, but there is a problem that abrasion resistance and flex resistance are deteriorated. Further, when it is used as a single polyurethane resin having a number average molecular weight of 100,000 to 130,000, scratch resistance is not sufficient, and tack is generated, which causes a problem in sewing and other process passability.
【0017】また数平均分子量10万〜13万のポリウ
レタン樹脂と数平均分子量2万〜10万のポリウレタン
樹脂のブレンドの場合、タックが残るといった欠点があ
り、数平均分子量10万〜13万のポリウレタン樹脂と
数平均分子量13万〜28万のポリウレタン樹脂のブレ
ンドの場合、耐屈曲性が悪くなるといった欠点がある。
また、数平均分子量が2万よりも小さいポリウレタン樹
脂と数平均分子量13万〜28万のポリウレタン樹脂の
ブレンドの場合もタックが残ってしまうという欠点があ
り、数平均分子量が28万よりも大きいポリウレタン樹
脂のブレンドの場合にも耐屈曲性が悪くなってしまう欠
点がある。よってブレンドするポリウレタン樹脂は数平
均分子量が2万〜10万の2液型ポリウレタン樹脂と数
平均分子量が13万〜28万の2液型ポリウレタン樹脂
であり、さらに該ポリウレタンのブレンド樹脂比率(重
量)(a)/(b)は0.05〜4の範囲が好ましく、
より好ましくは(a)/(b)が0.2〜2の割合でブ
レンドされたものである。なお、該ブレンド樹脂はクレ
ームの範囲外の分子量分布をもつ樹脂、例えばポリウレ
タン系の顔料インク等が樹脂全体の20重量%以内で添
加されても効果において左右されるものではない。Further, in the case of a blend of a polyurethane resin having a number average molecular weight of 100,000 to 130,000 and a polyurethane resin having a number average molecular weight of 20,000 to 100,000, there is a drawback that tack remains, and a polyurethane having a number average molecular weight of 100,000 to 130,000 is used. In the case of a blend of a resin and a polyurethane resin having a number average molecular weight of 130,000 to 280,000, there is a drawback that the bending resistance becomes poor.
Also, in the case of a blend of a polyurethane resin having a number average molecular weight of less than 20,000 and a polyurethane resin having a number average molecular weight of 130,000 to 280,000, there is a drawback that tack remains, and a polyurethane having a number average molecular weight of more than 280,000 is present. Even in the case of blending resins, there is a drawback that the bending resistance becomes poor. Accordingly, the polyurethane resins to be blended are a two-component polyurethane resin having a number average molecular weight of 20,000 to 100,000 and a two-component polyurethane resin having a number average molecular weight of 130,000 to 280,000, and the blending resin ratio (weight) of the polyurethane. (A) / (b) is preferably in the range of 0.05 to 4,
More preferably, (a) / (b) is blended at a ratio of 0.2 to 2. The blended resin does not affect the effect even if a resin having a molecular weight distribution outside the claimed range, such as a polyurethane-based pigment ink, is added within 20% by weight of the total resin.
【0018】添加するポリイソシアネート硬化剤として
は、トリメチロールプロパン(TMP)とトリレンジイ
ソシアネート(TDI)のアダクト体、TMPと4,
4’−メチレンビス(シクロヘキシルイソシアネート)
(HMDI)のアダクト体、TMPとHDIのアダクト
体、TMPとIPDIのアダクト体、HMDIの三量体
等の有機ポリイソシアネートが挙げられる。本発明に用
いられる有機ポリイソシアネートは2種以上の異なる有
機ポリイソシアネートを併用しても良く、特に脂肪族系
または脂環系ポリイソシアネートに芳香族系ポリイソシ
アネートを併用しても良い。添加量はポリウレタン樹脂
溶液に対しポリイソシアネート硬化剤を固形分重量比で
10%より少ないと耐擦過傷性および耐摩耗性が悪くな
り、75%を超えると耐屈曲性が悪くなるため、10〜
75%の範囲が良い。さらに好ましくは、20〜50%
の範囲である。また必要に応じて硬化剤の反応を阻害し
ない範囲で酸化防止剤、紫外線吸収剤、顔料、染料、界
面活性剤、帯電防止剤、難燃剤、粘着防止剤、充填剤等
の各種添加剤やコラーゲン粉末等を添加することもでき
る。As the polyisocyanate curing agent to be added, an adduct of trimethylolpropane (TMP) and tolylene diisocyanate (TDI), TMP and 4,
4'-methylenebis (cyclohexyl isocyanate)
Examples include organic polyisocyanates such as (HMDI) adduct, TMP and HDI adduct, TMP and IPDI adduct, and HMDI trimer. As the organic polyisocyanate used in the present invention, two or more different organic polyisocyanates may be used in combination, and in particular, an aliphatic or alicyclic polyisocyanate may be used in combination with an aromatic polyisocyanate. If the amount of polyisocyanate curing agent added to the polyurethane resin solution is less than 10% by weight of the solid content, the abrasion resistance and abrasion resistance will deteriorate, and if it exceeds 75%, the bending resistance will deteriorate.
A range of 75% is good. More preferably, 20 to 50%
Is the range. If necessary, various additives such as antioxidants, ultraviolet absorbers, pigments, dyes, surfactants, antistatic agents, flame retardants, anti-adhesives, fillers, etc. and collagen within a range that does not hinder the reaction of the curing agent. Powder or the like can also be added.
【0019】中間層(D)、接着層(B)を構成するポ
リウレタンの種類は、ポリエステル系、ポリエーテル
系、ポリカーボネート系あるいはそれらのブレンドまた
は変性体があるが、特に限定するものではなく既存のポ
リウレタン樹脂で良い。また、中間層(D)を設ける目
的は、造面層の厚み調整にあり、必ずしも設ける必要は
ない。接着層は、基体層(A)と層(C)を、或いは基
体層(A)と中間層(D)を接着するためのものであ
る。The type of polyurethane constituting the intermediate layer (D) and the adhesive layer (B) may be polyester type, polyether type, polycarbonate type, or blends or modified products thereof, but the present invention is not particularly limited. Polyurethane resin is good. Further, the purpose of providing the intermediate layer (D) is to adjust the thickness of the face-making layer and is not always necessary. The adhesive layer is for bonding the base layer (A) and the layer (C) or the base layer (A) and the intermediate layer (D).
【0020】コーテイング層の製造方法としては、ポリ
オレフィン系樹脂をコーテイングした離型紙上にポリウ
レタン樹脂(c)を塗布する方法を用いるのが好まし
い。他に最表面にアルキッド系樹脂、アミノアクリレー
ト系樹脂、アクリル系樹脂のコーテイングした離型紙が
あるが、これらの離型紙は本発明において、コーティン
グ樹脂との密着性が良すぎるため剥離しづらいといった
欠点がある。よって、離型紙は最表面コーテイング層が
ポリオレフィン系樹脂によるものが本発明においては好
ましい。As a method for producing the coating layer, it is preferable to use a method in which a polyurethane resin (c) is applied onto a release paper coated with a polyolefin resin. In addition, there are release papers coated with alkyd resin, amino acrylate resin, acrylic resin on the outermost surface, but these release papers in the present invention have the disadvantage that they are difficult to peel off because they have too good adhesion with the coating resin. There is. Therefore, it is preferable in the present invention that the outermost surface coating layer of the release paper is made of polyolefin resin.
【0021】塗布方法は、離型紙上にナイフコーター、
コンマコーター、ロールコーター、リバースコーター、
ロータリースクリーンコーターなどの手段によって塗布
する方法が用いられる。表面層(C)の乾燥後の厚みは
5μm〜100μm、好ましくは10μm〜50μmで
ある。5μm以下の場合には耐摩耗性が悪くなるという
問題があり、100μmを越える場合には表面が勝ちす
ぎて風合いが悪くなるという問題がある。また乾燥後の
最表面層(C)から接着層(B)までのトータル乾式造
面層の厚みとしては10μm〜200μmが好ましく、
特に50μm〜100μmが好ましい。膜厚が10μm
未満になると塗布ムラが発生する場合があり、膜厚が2
00μmを越えると風合いが硬くなる。The coating method is a knife coater on release paper,
Comma coater, roll coater, reverse coater,
A method of applying by a means such as a rotary screen coater is used. The thickness of the surface layer (C) after drying is 5 μm to 100 μm, preferably 10 μm to 50 μm. If it is 5 μm or less, there is a problem that the abrasion resistance is deteriorated, and if it is more than 100 μm, there is a problem that the surface is too strong and the texture is deteriorated. Further, the thickness of the total dry surface-forming layer from the outermost surface layer (C) to the adhesive layer (B) after drying is preferably 10 μm to 200 μm,
Particularly, 50 μm to 100 μm is preferable. Film thickness is 10 μm
If it is less than the range, uneven coating may occur, and the film thickness is 2
If it exceeds 00 μm, the texture becomes hard.
【0022】[0022]
【実施例】以下本発明の実施態様を具体的な実施例によ
り説明するが、本発明はこれら実施例に限定されるもの
ではない。なお、実施例中の部及び%はことわりのない
限り重量に関するものである。また以下の実施例及び比
較例において、耐擦過傷性、耐摩耗性、耐屈曲性、滑り
性の測定または評価は以下の方法に従って行った。EXAMPLES The embodiments of the present invention will be described below with reference to specific examples, but the present invention is not limited to these examples. Parts and% in the examples relate to weight unless otherwise specified. Further, in the following examples and comparative examples, the scratch resistance, abrasion resistance, flex resistance and slippage were measured or evaluated according to the following methods.
【0023】〔耐擦過傷性〕耐擦過傷性は、実施例およ
び比較例で得られた皮革様シートに対し、爪で約2kg
の荷重が掛かるように調整して時速約30〜50kmの
スピードでこすった後の白化傷の状態を判定した。白化
傷の状態評価は次に示す通りである。
○:白化傷無し。 △:白化傷薄く見える。 ×:白化
傷目立つ。[Scratch resistance] The scratch resistance of the leather-like sheets obtained in Examples and Comparative Examples is about 2 kg with nails.
The condition of whitening scratches after rubbing at a speed of about 30 to 50 km per hour was determined by adjusting so as to apply the load. The condition of whitening scratches is evaluated as follows. ◯: No whitening scratches. B: Whitening scratches appear thin. X: Whitening scratches are noticeable.
【0024】〔耐摩耗減量〕耐摩耗減量はテーバー磨耗
試験(JIS K7204)に従って測定した。すなわ
ち、実施例および比較例で得られた皮革様シートより直
径12cmの円形の試験片を切り出した。この円形試験
片の造面側に摩耗輪(Hー22)を当て、荷重1kgf
で円形の試験片を1000回転させて摩耗試験を行い、
摩耗試験の前の試験片の重量から摩耗試験後の試験片の
重量を差し引いて、テーバー摩耗量(摩耗によって減少
した重量)mgを求めた。[Abrasion Resistance Reduction] The abrasion resistance reduction was measured according to the Taber abrasion test (JIS K7204). That is, a circular test piece having a diameter of 12 cm was cut out from the leather-like sheet obtained in each of Examples and Comparative Examples. A wear wheel (H-22) is applied to the surface of this circular test piece to produce a load of 1 kgf.
A circular test piece is rotated 1000 times to perform a wear test,
The Taber abrasion amount (weight reduced by abrasion) mg was obtained by subtracting the weight of the specimen after the abrasion test from the weight of the specimen before the abrasion test.
【0025】〔耐屈曲性〕耐屈曲性は、FLEXO試験
法(JIS K6545)による判定。[Flex resistance] Flex resistance is determined by the FLEXO test method (JIS K6545).
【0026】〔滑り性〕滑り性は手で触った感触で、ド
ライタッチの場合が良好、若干タックがある場合をやや
不良、タックがある場合を不良とした。[Slipping Property] Sliding property is a touch feeling with a hand, good for dry touch, good for slight tack, and bad for tack.
【0027】実施例1
基体層(A)として、6−ナイロンを100部とポリエ
チレン100部を混合紡糸した後、延伸、捲縮及びカッ
トして、6−ナイロンが島成分となっている4drの原
綿を作製した。この原綿からランダムウエーバーによっ
てウエブを作り、ニードルパンチを行い430g/m2
の絡合不織布を作った。ついでポリビニルアルコール水
溶液に浸漬し、乾燥後更に135℃で熱処理をし、海成
分であるポリエチレンを融着せしめ硬いシートを作っ
た。その後、ポリエチレン・プロピレンアジペートグリ
コール/4、4−ジフェニルメタンジイソシアネート/
エチレングリコールを当量比で1/5/4で重合したポ
リウレタンエラストマーの13%のDMF溶液を含浸し
水70部及びDMF30部よりなる30℃の凝固浴中に
浸漬して湿式凝固した。引き続きこのシートをパークレ
ン中に浸漬して海成分のポリエチレンを抽出し、6−ナ
イロンの極細繊維束(単繊維の平均デニール、0.01
デニール)の絡合内部に多孔質ポリウレタンエラストマ
ーを有する基体層(A)を得た。このシートは目付37
0g/m2、見掛け密度0.35g/cm3、厚み1mm
であった。Example 1 As a base layer (A), 100 parts of 6-nylon and 100 parts of polyethylene were mixed and spun, and then stretched, crimped and cut to give a 4 dr of 6-nylon as an island component. Raw cotton was produced. A web is made from this raw cotton by a random weber and needle punched to 430 g / m 2.
Made entangled non-woven fabric. Then, it was dipped in an aqueous solution of polyvinyl alcohol, dried and further heat-treated at 135 ° C. to fuse polyethylene as a sea component to form a hard sheet. After that, polyethylene / propylene adipate glycol / 4,4-diphenylmethane diisocyanate /
A 13% DMF solution of a polyurethane elastomer obtained by polymerizing ethylene glycol at an equivalent ratio of ⅕ was impregnated and immersed in a coagulation bath of 70 parts of water and 30 parts of DMF at 30 ° C. for wet coagulation. Subsequently, this sheet was immersed in Perkren to extract polyethylene as a sea component, and an ultrafine fiber bundle of 6-nylon (average denier of single fiber, 0.01
A base layer (A) having a porous polyurethane elastomer inside the entanglement of denier) was obtained. This sheet has a basis weight of 37
0 g / m 2 , apparent density 0.35 g / cm 3 , thickness 1 mm
Met.
【0028】次に乾式造面を行うが、表面層(C)を構
成するポリウレタン樹脂溶液を下記の要領にて作製し
た。2液型ポリウレタン(a)(ポリオール成分として
1,6−ヘキサンポリカーボネートポリオールと、ジイ
ソシアネート化合物としてトリレンジイソシアネート
(TDI)と、鎖伸長剤としてエチレングリコールから
重合した固形分濃度70%のジメチルホルムアミド(D
MF)溶液、数平均分子量:7万)を10部と2液型ポ
リウレタン(b)(ポリオール成分として1,6−ヘキ
サンポリカーボネートポリオールと、ジイソシアネート
化合物としてトリレンジイソシアネート(TDI)と、
鎖伸長剤としてエチレングリコールから重合した固形分
濃度が30%のDMF溶液、数平均分子量17万)90
部をブレンドした。このブレンドもののブレンド比率は
(a)/(b)が0.26であった。Next, a dry surface is formed, and a polyurethane resin solution constituting the surface layer (C) was prepared in the following manner. Two-component polyurethane (a) (1,6-hexane polycarbonate polyol as a polyol component, tolylene diisocyanate (TDI) as a diisocyanate compound, and dimethylformamide (D) having a solid content concentration of 70% polymerized from ethylene glycol as a chain extender.
MF) solution, 10 parts of number average molecular weight: 70,000, two-component polyurethane (b) (1,6-hexane polycarbonate polyol as a polyol component, and tolylene diisocyanate (TDI) as a diisocyanate compound,
Polymerized from ethylene glycol as a chain extender, DMF solution with a solid concentration of 30%, number average molecular weight 170,000) 90
Parts were blended. The blend ratio (a) / (b) of this blend was 0.26.
【0029】このブレンド樹脂(c)100部に対し、
顔料として酸化チタン粉末を6部、ポリイソシアネート
硬化剤(d)(TMPとHDIのアダクト体で固形分濃
度75%酢酸エチル溶液)を15部(ポリウレタン樹脂
に対する硬化剤の固形分比率33%)、硬化促進剤とし
てアミン系触媒(e)(固形分4%)5部、希釈溶剤と
してDMF40部、メチルエチルケトン(MEK)40
部添加し、均一に混合してコーティング液を調整し、離
型紙(旭ロール社製AR−60SG(表面がポリオレフ
ィン系樹脂によりコーテイングしたもの)上にコンマコ
ーターにて100g/m2の塗布量で均一に塗布し、1
00〜130℃の乾燥炉で1分間乾燥して皮膜を得た。With respect to 100 parts of this blended resin (c),
6 parts of titanium oxide powder as a pigment, 15 parts of polyisocyanate curing agent (d) (75% solid content concentration of TMP and HDI adduct in ethyl acetate) (33% solid content ratio of curing agent to polyurethane resin), Amine catalyst (e) (4% solid content) 5 parts as a curing accelerator, DMF 40 parts as a diluting solvent, methyl ethyl ketone (MEK) 40
Parts, and mixed uniformly to adjust the coating liquid, and coated on a release paper (AR-60SG manufactured by Asahi Roll Co., whose surface is coated with a polyolefin resin) with a comma coater at a coating amount of 100 g / m 2. Apply evenly, 1
A film was obtained by drying for 1 minute in a drying oven at 00 to 130 ° C.
【0030】そしてその上に接着層(B)として2液型
ポリウレタン(a)を100部、酸化チタン粉末を6
部、ポリイソシアネート硬化剤(d)を8部、アミン系
触媒(e)を5部、DMFを15部、MEKを15部添
加し均一に混合して更に表面層上にコンマコーターにて
100g/m2の塗布量で均一に塗布し、70℃の乾燥
炉で1分間乾燥し皮膜を得た。そして、乾燥直後のまだ
粘着性を有する状態で該シート上にドライラミネートに
て前記基体層(A)をプレスして貼り合わせた。その後
60℃で48時間放置してから離型紙をはがし、目的の
皮革様シートを得た。得られたシートは表1に示すとお
り、耐屈曲性、耐擦過傷性および耐摩耗性が優れ、かつ
滑り性の良好なものであった。Then, 100 parts of two-component polyurethane (a) as an adhesive layer (B) and 6 parts of titanium oxide powder were formed thereon.
Parts, 8 parts of the polyisocyanate curing agent (d), 5 parts of the amine-based catalyst (e), 15 parts of DMF and 15 parts of MEK and uniformly mixed, and further 100 g / commercial on the surface layer with a comma coater. A coating amount of m 2 was applied uniformly, followed by drying for 1 minute in a drying oven at 70 ° C. to obtain a film. Then, the base layer (A) was pressed and laminated on the sheet by dry lamination immediately after drying in a state of having tackiness. Then, after leaving it at 60 ° C. for 48 hours, the release paper was peeled off to obtain a desired leather-like sheet. As shown in Table 1, the obtained sheet was excellent in bending resistance, abrasion resistance and abrasion resistance, and had good slidability.
【0031】比較例1
実施例1の基体層(A)を使用し、乾式造面を下記の要
領にて行った。表面層を構成するポリウレタン樹脂溶液
として、実施例1に対し2液型ポリウレタン(b)をブ
レンドせずに2液型ポリウレタン(a)100部に対
し、顔料として酸化チタン粉末6部、ポリイソシアネー
ト硬化剤(d)15部、硬化促進剤としてアミン系触媒
(e)5部、希釈溶剤としてDMF40部及びメチルエ
チルケトン(MEK)40部を添加し、均一に混合して
コーテイング液を調整し、前記離型紙上にコンマコータ
ーにてこのコーティング液を100g/m2の塗布量で
均一に塗布し、100〜130℃の乾燥炉で1分間乾燥
して皮膜を得た。Comparative Example 1 The substrate layer (A) of Example 1 was used, and a dry-fabricated surface was formed as follows. As the polyurethane resin solution forming the surface layer, 100 parts of the two-component polyurethane (a) without blending the two-component polyurethane (b) with respect to Example 1, 6 parts of titanium oxide powder as a pigment, and polyisocyanate curing The release paper is prepared by adding 15 parts of the agent (d), 5 parts of the amine catalyst (e) as a curing accelerator, 40 parts of DMF and 40 parts of methyl ethyl ketone (MEK) as a diluting solvent, and uniformly mixing them to prepare a coating liquid. This coating solution was applied uniformly on the above with a comma coater at a coating amount of 100 g / m 2 , and dried in a drying oven at 100 to 130 ° C. for 1 minute to obtain a film.
【0032】そして、その上に接着層(B)として、2
液型ポリウレタン(a)100部、酸化チタン粉末6
部、ポリシソシアネート硬化剤(d)8部、アミン系触
媒(e)5部、DMF15部及びMEK15部からなる
均一混合液をコンマコーターにて100g/m2の塗布
量で均一に塗布し、70℃の乾燥炉で1分間乾燥し皮膜
を得た。そして乾燥直後のまだ粘着性を有する状態で該
シートにドライラミネートにて前記基体層(A)にプレ
スして貼り合わせた。その後60℃で48時間放置して
から離型紙を剥がし、皮革様シートを得た。得られたシ
ートは表1に示すとおり、耐屈曲性、耐擦過傷性および
耐摩耗性は良好であるが、滑り性の悪い粘着性のあるタ
ックとなり、目的のシートは得られなかった。Then, as an adhesive layer (B) thereon, 2
Liquid polyurethane (a) 100 parts, titanium oxide powder 6
Part, polyisocyanate curing agent (d) 8 parts, amine-based catalyst (e) 5 parts, DMF 15 parts and MEK 15 parts were uniformly applied with a comma coater at an application amount of 100 g / m 2 . A film was obtained by drying for 1 minute in a drying oven at 70 ° C. Immediately after being dried, the sheet was dried and laminated on the base layer (A) by pressing on the base layer (A). After that, the release paper was peeled off after standing at 60 ° C. for 48 hours to obtain a leather-like sheet. As shown in Table 1, the obtained sheet had good bending resistance, abrasion resistance, and abrasion resistance, but had tackiness with poor slipperiness, and the intended sheet could not be obtained.
【0033】比較例2
実施例1の基体層(A)を使用し、乾式造面を下記の要
領にて行った。表面層(C)を構成するポリウレタン樹
脂溶液は、前記実施例1に対し2液型ポリウレタン
(a)をブレンドせずに、2液型ポリウレタン(b)1
00部に対し、顔料として酸化チタン粉末6部、ポリイ
ソシアネート硬化剤(d)15部、硬化促進剤としてア
ミン系触媒(e)5部、希釈溶剤としてDMF40部、
メチルエチルケトン(MEK)40部を添加し、均一に
混合してコーテイング液を調整し、前記離型紙上にコン
マコーターにて100g/m2を均一に塗布し、100
〜130℃の乾燥炉で1分間乾燥して皮膜を得た。そし
て、その上に、接着層(B)として、2液型ポリウレタ
ン(a)100部、酸化チタン粉末6部、ポリシソシア
ネート硬化剤(d)8部、アミン系触媒(e)5部、D
MF15部及びMEK15部からなる均一混合液をコン
マコーターにて100g/m2の塗布量で均一に塗布
し、70℃の乾燥炉で1分間乾燥し皮膜を得た。そして
乾燥直後の粘着性を有する状態で該シートにドライラミ
ネートにて前記基体層(A)にプレスして貼り合わせ
た。その後60℃で48時間放置してから離型紙を剥が
し、皮革様シートを得た。得られた皮革様シートは表1
に示すとおり、耐擦過傷性、耐摩耗性、最表面の滑り性
は良好であるが、耐屈曲性が不良となり、目的のシート
は得られなかった。Comparative Example 2 Using the substrate layer (A) of Example 1, a dry surface-making process was carried out in the following manner. The polyurethane resin solution constituting the surface layer (C) was prepared by blending the two-component polyurethane (a) with the two-component polyurethane (b) 1 in comparison with Example 1 described above.
To 00 parts, 6 parts titanium oxide powder as a pigment, 15 parts polyisocyanate curing agent (d), 5 parts amine catalyst (e) as a curing accelerator, 40 parts DMF as a diluting solvent,
40 parts of methyl ethyl ketone (MEK) was added and uniformly mixed to prepare a coating solution, and 100 g / m 2 was evenly applied onto the release paper with a comma coater.
A film was obtained by drying in a drying oven at ˜130 ° C. for 1 minute. Then, 100 parts of two-component polyurethane (a), 6 parts of titanium oxide powder, 8 parts of polycisocyanate curing agent (d), 5 parts of amine-based catalyst (e), D as an adhesive layer (B) thereon.
A uniform mixed solution consisting of 15 parts of MF and 15 parts of MEK was applied uniformly with a comma coater at a coating amount of 100 g / m 2 , and dried in a drying oven at 70 ° C. for 1 minute to obtain a film. Then, in the state of having the tackiness immediately after drying, the sheet was pressed and bonded to the base layer (A) by dry lamination. After that, the release paper was peeled off after standing at 60 ° C. for 48 hours to obtain a leather-like sheet. The leather-like sheet obtained is shown in Table 1.
As shown in, the abrasion resistance, the abrasion resistance, and the slipperiness of the outermost surface were good, but the bending resistance was poor, and the target sheet could not be obtained.
【0034】実施例2
実施例1の基体層(A)を使用し、乾式造面を下記の要
領にて行った。表面層を構成するポリウレタン樹脂溶液
は、2液型ポリウレタン(a)を10部と2液型ポリウ
レタン(b)を90部をブレンドした。このブレンドも
のブレンド比率は(a)/(b)が0.26である。こ
のブレンド樹脂(c)100部に対し顔料として酸化チ
タン粉末6部、ポリイソシアネート硬化剤(d)3部
(ポリウレタン樹脂に対する硬化剤の固形分比率6.6
%)とし、硬化剤の添加量は実施例1に対し極めて少な
い量とした。さらに、硬化促進剤としてアミン系触媒
(e)(固形分4%)5部、希釈溶剤としてDMF40
部、メチルエチルケトン(MEK)40部添加し均一に
混合してコーテイング液を調整し、前記離型紙上にコン
マコーターにて100g/m2の塗布量で均一に塗布
し、100〜130℃の乾燥炉で1分間乾燥して皮膜を
得た。そして、その上に接着層(B)として2液型ポリ
ウレタン(a)100部、酸化チタン粉末6部、ポリイ
ソシアネート硬化剤(d)8部、アミン系触媒(e)5
部、DMF15部、MEK15部からなる均一混合液を
コンマコーターにて100g/m2の塗布量で均一に塗
布し、70℃の乾燥炉で1分間乾燥し皮膜を得た。そし
て、乾燥直後の粘着性を有する状態で該シートにドライ
ラミネートにて前記基体層(A)にプレスして貼り合わ
せた。その後60℃で48時間放置してから離型紙をは
がし、目的の皮革様シートを得た。得られたシートは表
1に示すとおり、耐屈曲性は良好であるが、耐擦過傷
性、耐摩耗性および滑り性は必ずしも良くない皮革様シ
ートであった。Example 2 Using the substrate layer (A) of Example 1, a dry surface-making process was carried out as follows. The polyurethane resin solution forming the surface layer was prepared by blending 10 parts of the two-component polyurethane (a) and 90 parts of the two-component polyurethane (b). The blend ratio of this blend is (a) / (b) is 0.26. To 100 parts of this blended resin (c), 6 parts of titanium oxide powder as a pigment and 3 parts of polyisocyanate curing agent (d) (solid content ratio of curing agent to polyurethane resin 6.6) were used.
%), And the addition amount of the curing agent was set to be extremely smaller than that in Example 1. Furthermore, 5 parts of an amine-based catalyst (e) (solid content 4%) as a curing accelerator, and DMF40 as a diluting solvent
Parts, 40 parts of methyl ethyl ketone (MEK) are added and uniformly mixed to prepare a coating solution, and the release paper is evenly coated with a comma coater at a coating amount of 100 g / m 2 , and a drying oven at 100 to 130 ° C. And dried for 1 minute to obtain a film. Then, 2-component polyurethane (a) 100 parts as the adhesive layer (B) thereon, 6 parts of titanium oxide powder, poly Lee <br/> isocyanate curing agent (d) 8 parts of amine catalyst (e) 5
Part, DMF 15 parts, and MEK 15 parts were uniformly applied with a comma coater at an application amount of 100 g / m 2 , and dried in a drying oven at 70 ° C. for 1 minute to obtain a film. Then, in a state of having tackiness immediately after drying, the sheet was dry laminated and pressed onto the base layer (A) to be laminated. Then, after leaving it at 60 ° C. for 48 hours, the release paper was peeled off to obtain a desired leather-like sheet. As shown in Table 1, the obtained sheet was a leather-like sheet having good flex resistance but poor abrasion resistance, abrasion resistance and slipperiness.
【0035】実施例3
実施例1の基体層(A)を使用し、乾式造面を下記の要
領にて行った。表面層を構成するポリウレタン樹脂溶液
は、2液型ポリウレタン(a)を10部と2液型ポリウ
レタン(b)を90部をブレンドした。このブレンドも
ののブレンド比率は(a)/(b)が0.26である。
このブレンド樹脂(c)100部に対し顔料として酸化
チタン粉末6部、ポリイソシアネート硬化剤(d)50
部(ポリウレタン樹脂に対する硬化剤の固形分比率11
0%)とし、硬化剤の添加量は実施例1に対し極めて多
い量とした。さらに、硬化促進剤としてアミン系触媒
(e)(固形分4%)5部、希釈溶剤としてDMF40
部、メチルエチルケトン(MEK)40部を添加し均一
に混合した液を調整し、前記離型紙上にコンマコーター
にて100g/m2の塗布量で均一に塗布し、100〜
130℃の乾燥炉で1分間乾燥して皮膜を得た。そし
て、その上に、接着層(B)として、2液型ポリウレタ
ン(a)100部、酸化チタン粉末6部、ポリイソシア
ネート硬化剤(d)8部、アミン系触媒(e)5部、D
MF15部及びMEK15部からなる均一混合液をコン
マコーターにて100g/m2を均一に塗布し、70℃
の乾燥炉で1分間乾燥し皮膜を得た。そして、乾燥直後
の粘着性を有する状態で該シートにドライラミネートに
て前記基体層(A)にプレスして貼り合わせた。その後
60℃で48時間放置してから離型紙をはがし、目的の
皮革様シートを得た。得られたシートは表1に示すとお
り、耐擦過傷性、耐摩耗性および滑り性は良好である
が、耐屈曲性は十分良好とは言えない皮革様シートであ
った。Example 3 Using the substrate layer (A) of Example 1, a dry surface-making process was carried out in the following manner. The polyurethane resin solution forming the surface layer was prepared by blending 10 parts of the two-component polyurethane (a) and 90 parts of the two-component polyurethane (b). The blend ratio (a) / (b) of this blend is 0.26.
To 100 parts of this blended resin (c), 6 parts of titanium oxide powder as a pigment and 50 parts of polyisocyanate curing agent (d)
Part (solid content ratio of curing agent to polyurethane resin 11
0%), and the addition amount of the curing agent was set to an extremely large amount as compared with Example 1. Furthermore, 5 parts of an amine-based catalyst (e) (solid content 4%) as a curing accelerator, and DMF40 as a diluting solvent
Parts and 40 parts of methyl ethyl ketone (MEK) were added and uniformly mixed to prepare a solution, which was uniformly applied onto the release paper with a comma coater at an application amount of 100 g / m 2 ,
A film was obtained by drying for 1 minute in a drying oven at 130 ° C. Then, 100 parts of two-component polyurethane (a), 6 parts of titanium oxide powder, 8 parts of polyisocyanate curing agent (d), 5 parts of amine-based catalyst (e), and D as an adhesive layer (B) thereon.
A uniform mixed solution consisting of 15 parts of MF and 15 parts of MEK was evenly applied at 100 g / m 2 with a comma coater, and 70 ° C.
It was dried for 1 minute in the drying oven of No. 1 to obtain a film. Then, in a state of having tackiness immediately after drying, the sheet was dry laminated and pressed onto the base layer (A) to be laminated. Then, after leaving it at 60 ° C. for 48 hours, the release paper was peeled off to obtain a desired leather-like sheet. As shown in Table 1, the obtained sheet was a leather-like sheet having good abrasion resistance, abrasion resistance and slippage, but not sufficient flex resistance.
【0036】比較例3
実施例1の基体層(A)を使用し、乾式造面を下記の要
領にて行った。表面層(C)を構成するポリウレタン樹
脂溶液として、実施例1に対し2液型ポリウレタン
(f)(ポリオール成分として1,6−ヘキサンポリカ
ーボネートポリオールと、ジイソシアネート化合物とし
てトリレンジイソシアネート(TDI)と鎖伸長剤とし
てエチレングリコールから重合した固形分濃度が70%
のDMF溶液(数平均分子量11万)100部に対し、
顔料として酸化チタン粉末6部、ポリイソシアネート硬
化剤(d)、硬化促進剤としてアミン系触媒(e)5
部、希釈溶剤としてDMF40部、メチルエチルケトン
(MEK)40部を添加し均一に混合したコーテイング
液を前記離型紙上にコンマコーターにて塗布量100g
/m2で均一に塗布し、100〜130℃の乾燥炉で1
分間乾燥して皮膜を得た。そして、その上に接着層
(B)として、2液型ポリウレタン(a)100部、酸
化チタン粉末6部、ポリイソシアネート硬化剤(d)8
部、アミン系触媒(e)5部、DMF15部及びMEK
15部からなる均一溶液をコンマコーターにて塗布量1
00g/m2で均一に塗布し、70℃の乾燥炉で1分間
乾燥し皮膜を得た。そして、乾燥直後のまだ粘着性を有
する状態で該シートにドライラミネートにて前記基体層
(A)にプレスして貼り合わせた。その後60℃で48
時間放置してから離型紙をはがし、皮革様シートを得
た。得られたシートは表1に示すとおり、耐屈曲性、耐
摩耗性は良好であるが耐擦過傷性効果および滑り性効果
が満足されず、目的のシートは得られなかった。Comparative Example 3 Using the substrate layer (A) of Example 1, a dry surface-making process was carried out in the following manner. As a polyurethane resin solution constituting the surface layer (C), a two-component polyurethane (f) was prepared as in Example 1 (1,6-hexane polycarbonate polyol as a polyol component, tolylene diisocyanate (TDI) as a diisocyanate compound, and chain extension). 70% solid content polymerized from ethylene glycol as an agent
Of DMF solution (number average molecular weight 110,000) of
6 parts of titanium oxide powder as a pigment, polyisocyanate curing agent (d), amine catalyst (e) 5 as a curing accelerator
Parts, 40 parts of DMF as a diluting solvent, and 40 parts of methyl ethyl ketone (MEK) were added and uniformly mixed, and a coating liquid of 100 g was applied onto the release paper with a comma coater.
/ M 2 and apply evenly in a drying oven at 100-130 ° C.
After drying for a minute, a film was obtained. Then, 100 parts of two-component polyurethane (a), 6 parts of titanium oxide powder, and polyisocyanate curing agent (d) 8 as an adhesive layer (B) thereon.
Parts, 5 parts of amine-based catalyst (e), 15 parts of DMF and MEK
Apply 15 parts of homogeneous solution with comma coater
The coating was uniformly applied at 00 g / m 2 and dried in a drying oven at 70 ° C. for 1 minute to obtain a film. Immediately after drying, the sheet was dried and laminated on the base layer (A) by pressing and adhering to the sheet while still sticking. Then 48 at 60 ° C
After being left for a period of time, the release paper was peeled off to obtain a leather-like sheet. As shown in Table 1, the obtained sheet was good in flex resistance and abrasion resistance, but the scuff resistance effect and the slipping effect were not satisfied, and the intended sheet could not be obtained.
【0037】[0037]
【表1】 [Table 1]
【0038】総合評価方法においては以下に示した通
り。
○:良好、 △:やや不良、 ×:不良。The comprehensive evaluation method is as shown below. ◯: Good, Δ: Slightly bad, X: Bad.
【0039】[0039]
【発明の効果】本発明により、最表面の耐擦過性、耐摩
耗性、耐屈曲性および滑り性に優れた皮革様シートが得
られ、本発明の皮革様シートは、スポーツ用品、一般
靴、鞄、バックなどの袋物、衣料および衣料パーツ等に
使用することができる。EFFECTS OF THE INVENTION According to the present invention, a leather-like sheet having excellent scratch resistance, abrasion resistance, bending resistance and slipperiness on the outermost surface can be obtained, and the leather-like sheet of the present invention can be used for sports goods, general shoes, It can be used for bags, bags such as bags, clothing and clothing parts.
───────────────────────────────────────────────────── フロントページの続き (56)参考文献 特開 平6−81275(JP,A) 特開 平5−279967(JP,A) 特開 平5−222681(JP,A) 特開 平5−163684(JP,A) 特開 平5−163682(JP,A) 特開 平2−127574(JP,A) 特開 昭60−173180(JP,A) 特開 昭56−112579(JP,A) (58)調査した分野(Int.Cl.7,DB名) D06N 3/00 - 3/18 ─────────────────────────────────────────────────── ─── Continuation of front page (56) Reference JP-A-6-81275 (JP, A) JP-A-5-279967 (JP, A) JP-A-5-222681 (JP, A) JP-A-5- 163684 (JP, A) JP 5-163682 (JP, A) JP 2-127574 (JP, A) JP 60-173180 (JP, A) JP 56-112579 (JP, A) (58) Fields investigated (Int.Cl. 7 , DB name) D06N 3/00-3/18
Claims (6)
合体を含有した基体層(A)上に、ポリウレタン樹脂を
主体とする樹脂からなる接着剤層(B)を介して、数平
均分子量が2万〜10万の2液型ポリウレタン樹脂
(a)と数平均分子量が13万〜28万の2液型ポリウ
レタン樹脂(b)が、ポリイソシアネート系硬化剤によ
り架橋された樹脂からなる層(C)が積層されている皮
革様シート。1. A number average through a base layer (A) containing a polymer mainly composed of an elastic polymer in a fiber assembly, with an adhesive layer (B) composed of a resin mainly composed of a polyurethane resin interposed therebetween. A layer made of a resin in which a two-component polyurethane resin (a) having a molecular weight of 20,000 to 100,000 and a two-component polyurethane resin (b) having a number average molecular weight of 130,000 to 280,000 are crosslinked with a polyisocyanate curing agent. A leather-like sheet in which (C) is laminated.
(b)のブレンド重量比が0.05〜4である請求項1
記載の皮革様シート。2. The blend weight ratio of the polyurethane (a) and the polyurethane (b) is 0.05 to 4.
The leather-like sheet described.
ウレタン中間層(D)が設けられている請求項1記載の
皮革様シート。3. The leather-like sheet according to claim 1, wherein a polyurethane intermediate layer (D) is provided between the layer (C) and the adhesive layer (B).
リウレタン樹脂(a)と数平均分子量が13万〜28万
の2液型ポリウレタン樹脂(b)および該樹脂(a)と
(b)の合計重量に対して固形分比10〜75重量%の
ポリイソシアネート硬化剤を含むポリウレタン樹脂を離
型紙上に塗布し、乾燥して層(C)を形成した後、接着
層(B)を介して、繊維集合体に弾性重合体を主体とし
た重合体を含有した基体層(A)に貼着し硬化反応を行
わせた後、該離型紙を剥離することを特徴とする皮革様
シートの製造方法。4. A two-component polyurethane resin (a) having a number average molecular weight of 20,000 to 100,000, a two-component polyurethane resin (b) having a number average molecular weight of 130,000 to 280,000, and the resin (a) ( A polyurethane resin containing a polyisocyanate curing agent in a solid content ratio of 10 to 75% by weight based on the total weight of b) is applied on a release paper and dried to form a layer (C), and then an adhesive layer (B). The release paper is peeled off after being adhered to the base layer (A) containing a polymer mainly composed of an elastic polymer through a fiber to cause a curing reaction. Sheet manufacturing method.
(b)のブレンド重量比が0.05〜4の割合である請
求項4記載の製造方法。5. The method according to claim 4, wherein the blending weight ratio of the polyurethane (a) and the polyurethane (b) is 0.05 to 4.
レフィン系にしたものである請求項4記載の製造方法。6. The production method according to claim 4, wherein the outermost surface coating layer of the release paper is made of polyolefin.