JP2000314066A - Felt and its production, and binder for felt - Google Patents
Felt and its production, and binder for feltInfo
- Publication number
- JP2000314066A JP2000314066A JP12645199A JP12645199A JP2000314066A JP 2000314066 A JP2000314066 A JP 2000314066A JP 12645199 A JP12645199 A JP 12645199A JP 12645199 A JP12645199 A JP 12645199A JP 2000314066 A JP2000314066 A JP 2000314066A
- Authority
- JP
- Japan
- Prior art keywords
- felt
- binder
- weight
- mat
- product
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Withdrawn
Abstract
Description
【0001】[0001]
【発明の属する技術分野】本発明は、自動車、家電製
品、家具類の内装材、断熱材、吸音材、緩衝材などに用
いられるフェルトの製造方法に関するものであり、特
に、製造時の作業環境を良好とすることができるフェル
トの製造方法に関する。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method for producing felt used for automobiles, home appliances, furniture interior materials, heat insulating materials, sound absorbing materials, cushioning materials, and the like. The present invention relates to a method for producing a felt capable of improving the felt quality.
【0002】[0002]
【従来の技術】従来、フェルトの製造方法としては、次
のようなものがある。合成繊維などの基材繊維を細断
し、次いで取り扱いを容易化するためオイルなどを添加
し含液率を調整した後、フリースマシンによりフリース
とする。次いでこのフリースにバインダを加えて混合し
た後、混合物を加熱加圧成形してフェルトを得る。フェ
ルトとしては、車両内装(天井、床など)やエアコン用
断熱材に用いられるマットフェルト(密度約0.03〜
0.1g/cm3)と、車両ボンネット内面やエンジン
ルームなどに用いられるボードフェルト(密度約0.3
〜0.7g/cm3)が広く用いられている。上記バイ
ンダとしては、通常、粉末状のノボラック型フェノール
樹脂と、ヘキサメチレンテトラミンなどの硬化剤との混
合物などが用いられる。2. Description of the Related Art Conventionally, there are the following methods for manufacturing felt. A base fiber such as a synthetic fiber is shredded, and then oil or the like is added to facilitate the handling and the liquid content is adjusted. Next, a binder is added to the fleece and mixed, and then the mixture is heated and pressed to obtain a felt. As felt, mat felt used for vehicle interiors (ceilings, floors, etc.) and thermal insulation for air conditioners (density approx.
0.1 g / cm 3 ) and a board felt (density of about 0.3
0.70.7 g / cm 3 ) is widely used. As the binder, a mixture of a powdery novolak type phenol resin and a curing agent such as hexamethylenetetramine is usually used.
【0003】[0003]
【発明が解決しようとする課題】しかしながら、上記従
来技術では、製造時においてバインダを原因とする臭
気、粉塵が発生しやすく、作業環境の改善が要望されて
いた。また、バインダに由来する臭気が製品に残ること
があった。本発明は、上記事情に鑑みてなされたもの
で、その目的は、以下の通りである。 (1)製造の際の作業環境を良好とすることができるフ
ェルトの製造方法の提供。 (2)製品の臭気を抑えることができるフェルトの製造
方法の提供。However, in the above-mentioned prior art, odor and dust due to the binder are likely to be generated at the time of manufacturing, and there has been a demand for improvement of the working environment. Moreover, the odor derived from the binder sometimes remained in the product. The present invention has been made in view of the above circumstances, and has the following objects. (1) To provide a felt manufacturing method capable of improving the working environment during manufacturing. (2) To provide a felt manufacturing method capable of suppressing the odor of a product.
【0004】[0004]
【課題を解決するための手段】上記課題は、液状バイン
ダを基材繊維に添加してフリースとし、このフリースを
加熱成形するフェルトの製造方法によって解決すること
ができる。液状バインダとしては、フェノール樹脂が安
価であり、しかも臭気の発生が少ないため、コスト面お
よび作業環境の面から好ましい。フェノール樹脂として
は、レゾール型フェノール樹脂を用いるのが好ましい。
また本発明のフェルトは、上記フェルトの製造方法によ
って得られたものであることを特徴とするものである。
また本発明のフェルト用バインダは、上記方法に用いら
れるバインダであって、液状物であることを特徴とする
ものである。The above object can be attained by a method of manufacturing a felt by adding a liquid binder to a base fiber to form a fleece and heat-forming the fleece. As the liquid binder, a phenol resin is inexpensive and generates little odor, so that it is preferable in terms of cost and working environment. It is preferable to use a resol type phenol resin as the phenol resin.
Further, the felt of the present invention is obtained by the above-described method for producing felt.
The felt binder of the present invention is a binder used in the above method, and is characterized by being a liquid material.
【0005】[0005]
【発明の実施の形態】以下、本発明のフェルトの製造方
法の一例を詳しく説明する。まず、基材繊維を用意す
る。この基材繊維としては、ナイロン繊維、ビニロン繊
維、ポリエステル繊維、ポリプロピレン繊維、レーヨン
繊維などの合成繊維や、木質繊維、綿繊維、麻繊維、ケ
ナフ繊維などの天然繊維を使用することができる。また
この他、ガラス繊維、炭素繊維などの無機繊維を使用す
ることもできる。これら繊維は単独で用いてもよいし、
これらのうち2種以上を使用してもよい。基材繊維とし
ては、上記繊維からなる縫製落ちの布(チップ)などを
使用できる。BEST MODE FOR CARRYING OUT THE INVENTION Hereinafter, an example of a method for producing felt of the present invention will be described in detail. First, a base fiber is prepared. As the base fiber, synthetic fibers such as nylon fiber, vinylon fiber, polyester fiber, polypropylene fiber and rayon fiber, and natural fibers such as wood fiber, cotton fiber, hemp fiber and kenaf fiber can be used. In addition, inorganic fibers such as glass fiber and carbon fiber can also be used. These fibers may be used alone,
Two or more of these may be used. As the base fiber, a sewn-off cloth (chip) made of the above fiber can be used.
【0006】上記基材繊維を必要に応じて細断した後、
この基材繊維に、液状バインダを添加、混合する。液状
バインダとは、液体バインダのほか、固形物(粉末な
ど)を必要に応じて乳化剤などを添加して分散媒(水な
ど)中に懸濁し液状としたものや、上記固形物を溶媒中
に溶解し液状としたものを含む。After shredding the base fiber as required,
A liquid binder is added to and mixed with the base fiber. The liquid binder is a liquid binder, a solid (powder, etc.) added with an emulsifier or the like, if necessary, and suspended in a dispersion medium (water, etc.) to form a liquid, or the above solid in a solvent. Including those dissolved and liquid.
【0007】液状バインダとしては、フェノール樹脂、
メラミン樹脂、ユリア樹脂、ウレタン樹脂、ポリイミド
樹脂、ポリアミド樹脂、エポキシ樹脂、ポリエステル樹
脂、アクリル樹脂、酢酸ビニル樹脂、塩化ビニル樹脂、
塩化ビニリデン樹脂、天然系樹脂(セルロース、ロジン
など)、および石油系樹脂のうち1種以上を含むものを
用いることができる。これらの樹脂に用いられる硬化剤
としては、ヘキサメチレンテトラミン、有機ポリアミン
(トリエチレンテトラミン、トリエタノールアミン等)
などを使用しない方が、加熱時における有臭ガス、煙の
発生が少なくなる。上記樹脂のなかでも、フェノール樹
脂、メラミン樹脂、ユリア樹脂、ポリイミド樹脂、塩化
ビニル樹脂、および塩化ビニリデン樹脂のうち1種以上
を含むものを用いると、フェルト製品に難燃性を付与す
ることができるため好ましい。特に、フェノール樹脂
は、安価であり、しかも臭気の発生が少ないため、コス
ト面および作業環境の面から好ましい。As the liquid binder, phenol resin,
Melamine resin, urea resin, urethane resin, polyimide resin, polyamide resin, epoxy resin, polyester resin, acrylic resin, vinyl acetate resin, vinyl chloride resin,
A resin containing at least one of vinylidene chloride resin, natural resin (such as cellulose and rosin), and petroleum resin can be used. Hardening agents used for these resins include hexamethylenetetramine and organic polyamines (triethylenetetramine, triethanolamine, etc.)
The use of such a method reduces the generation of odorous gas and smoke during heating. Among the above resins, a phenol resin, a melamine resin, a urea resin, a polyimide resin, a vinyl chloride resin, and a resin containing at least one of vinylidene chloride resins can impart flame retardancy to a felt product. Therefore, it is preferable. In particular, phenol resins are preferable in terms of cost and working environment because they are inexpensive and generate little odor.
【0008】上記フェノール樹脂含有バインダとして
は、アルカリ触媒、例えば水酸化ナトリウム、水酸化カ
リウムなどの存在下で、フェノールとホルムアルデヒド
を、フェノール/ホルムアルデヒドのモル比が1/1.
0〜4.0の条件で反応させることにより得られた液状
物(レゾール型フェノール樹脂バインダ)、または上記
反応により得られた固形物(レゾール型フェノール樹脂
バインダ)の分散液を使用することができる。該分散液
を使用する場合には、均一な分散液を得るために、液状
バインダに対して3〜10重量%の乳化剤などの添加剤
を添加してもよい。乳化剤としては、アニオン系、カチ
オン系、ノニオン系などを用いることができる。As the phenol resin-containing binder, phenol and formaldehyde are used in the presence of an alkali catalyst such as sodium hydroxide or potassium hydroxide, and the phenol / formaldehyde molar ratio is 1 / 1.1.
A liquid (resole-type phenol resin binder) obtained by reacting under the conditions of 0 to 4.0 or a dispersion of a solid (resole-type phenol resin binder) obtained by the above reaction can be used. . When the dispersion is used, 3 to 10% by weight of an additive such as an emulsifier may be added to the liquid binder in order to obtain a uniform dispersion. As the emulsifier, an anionic, cationic, nonionic or the like can be used.
【0009】上記製法により得られた液状バインダとし
ては、遊離フェノール含有量が5重量%未満、遊離ホル
ムアルデヒド含有量が0.5重量%未満であるものを用
いるのが好ましい。遊離フェノール含有量が5重量%以
上、もしくは遊離ホルムアルデヒド含有量が1%以上で
あると、液状バインダを毒劇物として扱うことが必要と
なり取り扱いが難しくなる。また遊離ホルムアルデヒド
含有量が0.5重量%以上であると臭気が増加する。As the liquid binder obtained by the above-mentioned method, it is preferable to use a liquid binder having a free phenol content of less than 5% by weight and a free formaldehyde content of less than 0.5% by weight. When the free phenol content is 5% by weight or more or the free formaldehyde content is 1% or more, it is necessary to treat the liquid binder as a poisonous substance, which makes handling difficult. When the free formaldehyde content is 0.5% by weight or more, the odor increases.
【0010】また液状バインダとしては、液状ノボラッ
ク型フェノール樹脂バインダを用いることもできる。こ
の液状ノボラック型フェノール樹脂バインダとしては、
酸性触媒、例えば硫酸、塩酸などの存在下で、フェノー
ルとホルムアルデヒドを、フェノール/ホルムアルデヒ
ドのモル比が1/0.5〜0.9の条件で反応させるこ
とにより得られた固形物と、硬化剤としてのイソシアネ
ート化合物などの求水酸基の官能基(−NCO等)を含
む化合物との混合物の分散液または溶液を使用すること
ができる。上記硬化剤は、ヘキサメチレンテトラミンな
どの硬化剤に比べ加熱時における有臭ガス、煙の発生が
少ない。As the liquid binder, a liquid novolak type phenol resin binder can be used. As this liquid novolak type phenolic resin binder,
A solid obtained by reacting phenol and formaldehyde in the presence of an acidic catalyst such as sulfuric acid or hydrochloric acid at a phenol / formaldehyde molar ratio of 1 / 0.5 to 0.9; A dispersion or solution of a mixture with a compound containing a functional group of a hydroxyl group (such as -NCO) such as an isocyanate compound can be used. The curing agent generates less odorous gas and smoke when heated than a curing agent such as hexamethylenetetramine.
【0011】液状バインダの基材繊維に対する添加量
は、目的とするフェルト製品の種類、求められる強度や
表面状態などによって適宜設定される。マットフェルト
を製造する場合には、上記液状バインダの添加量は、基
材繊維100重量部に対して、固形分として5〜30重
量部、好ましくは7〜15重量部とするのが好適であ
る。この添加量が5重量部未満であると、フェルト製品
中で基材繊維どうしが十分に結合せず製品の強度が低下
する。また添加量が30重量部を越えると、製品が触感
や吸音性などの点で劣るものとなりやすい。またボード
フェルトを製造する場合には、液状バインダの添加量
は、基材繊維100重量部に対して、固形分として20
〜40重量部、好ましくは25〜35重量部とするのが
好適である。この添加量が20重量部未満であると、フ
ェルト製品中で基材繊維どうしが十分に結合せず製品の
強度が低下する。また添加量が40重量部を越えると、
製品が吸音性などの点で劣るものとなり、経済的に不利
となる。The amount of the liquid binder to be added to the base fiber is appropriately set according to the type of the desired felt product, the required strength and the surface condition, and the like. When producing a mat felt, the amount of the liquid binder to be added is preferably 5 to 30 parts by weight, preferably 7 to 15 parts by weight as a solid content with respect to 100 parts by weight of the base fiber. . If the amount is less than 5 parts by weight, the base fibers in the felt product are not sufficiently bonded to each other and the strength of the product is reduced. If the amount exceeds 30 parts by weight, the product tends to be inferior in terms of tactile sensation and sound absorption. When manufacturing board felt, the amount of the liquid binder to be added is 20 parts by weight based on 100 parts by weight of the base fiber.
The amount is preferably from 40 to 40 parts by weight, preferably from 25 to 35 parts by weight. When the addition amount is less than 20 parts by weight, the base fibers are not sufficiently bonded to each other in the felt product, and the strength of the product is reduced. When the amount exceeds 40 parts by weight,
The product is inferior in terms of sound absorption and the like, which is economically disadvantageous.
【0012】次いで、上記基材繊維と液状バインダの混
合物を、フリースマシンを用いて解繊し、フリースを得
る。この混合物およびフリースは室温での長期保存(1
〜5ヶ月)が可能である。Next, the mixture of the base fiber and the liquid binder is defibrated using a fleece machine to obtain a fleece. The mixture and the fleece are stored at room temperature for a long time (1
~ 5 months) is possible.
【0013】次に、得られたフリースを、フォーミング
装置により堆積させるフォーミングを行い、マットを得
る。マットフェルトを製造する場合には、上記マット
を、好ましくは200〜250℃の条件で2〜3分間加
熱して所定厚さのマットフェルトを得る。ボードフェル
トの場合には、上記マットを、好ましくは150〜20
0℃の条件で2〜3分間加熱して嵩高マットを得た後、
この嵩高マットを、加熱手段を備えたプレス装置により
所定の形状に加熱成形し、フェルト製品を得る。この加
熱成形時の温度条件は180〜250℃とするのが好ま
しい。また成形時の圧力条件は、10〜50kg/cm
2とするのが好ましい。液状バインダとして加熱により
硬化する性質を有するレゾール型フェノール樹脂含有バ
インダを用いる場合には、硬化剤を添加しなくても成形
が可能である。Next, forming is performed by depositing the obtained fleece by a forming apparatus to obtain a mat. When producing a mat felt, the above mat is preferably heated at 200 to 250 ° C. for 2 to 3 minutes to obtain a mat felt having a predetermined thickness. In the case of board felt, the mat is preferably used for 150 to 20 pieces.
After heating for 2 to 3 minutes at 0 ° C. to obtain a bulky mat,
The bulky mat is heated and formed into a predetermined shape by a press device provided with a heating means to obtain a felt product. It is preferable that the temperature condition at the time of the heat molding be 180 to 250 ° C. The pressure condition during molding is 10 to 50 kg / cm.
Preferably it is 2 . When a resol-type phenol resin-containing binder having a property of being cured by heating is used as the liquid binder, molding can be performed without adding a curing agent.
【0014】上記フェルトの製造方法にあっては、以下
に示す効果を得ることができる。 (1)バインダが液状であるため、従来用いられている
固形(粉末)バインダを用いた場合のように添加の際に
バインダが粉塵となって飛散することがなく、作業環境
を良好に保つことができる。またバインダの一部が飛散
により失われるのを防ぎ、バインダの利用効率を高め、
材料コスト削減を可能とすることができる。またバイン
ダの添加によりフリースの含液率を高め、フリースを取
り扱いやすい状態とすることができるため、含液率調整
用オイルなどを加えて繊維中の含液率を調整する工程を
不要とし、製造工程を簡略化することができる。このた
め、生産効率を高めるとともに、製造コストを低廉化す
ることが可能となる。 (2)硬化剤として、加熱時にホルムアルデヒド、アン
モニアなどのガスが発生しやすいヘキサメチレンテトラ
ミンを使用しないため、製造時において、硬化剤を原因
とする悪臭や、成形工程において硬化剤が加熱されるこ
とにより煙が発生するのを防ぐことができ、作業環境の
悪化を防ぐことができる。また、この硬化剤を原因とす
る臭気が製品に残るのを防ぎ、製品の臭気を抑えること
ができる。このため、製品を、臭気が閉鎖空間内に滞留
し問題となりやすい用途、例えば自動車の内装材として
使用する場合にも、製品が利用者に不快感を与えるのを
防ぐことができる。 (3)液状バインダとして、加熱により硬化する性質を
有するレゾール型フェノール樹脂バインダを用いること
によって、硬化剤を不要とし、材料コスト削減を図ると
ともに、硬化剤を原因とする悪臭を防ぐことができる。
また遊離ホルムアルデヒド含有量が低い(例えば0.5
重量%未満)レゾール型フェノール樹脂バインダを用い
ることによって、製品からのホルムアルデヒド放散量を
低く抑え、利用者が不快感を感じたり健康を悪化させる
のを防ぐことができる。According to the above felt manufacturing method, the following effects can be obtained. (1) Since the binder is in a liquid state, the binder is not scattered as dust when added as in the case of using a conventionally used solid (powder) binder, and the working environment is kept good. Can be. In addition, we prevent part of binder from being lost by scattering and improve the use efficiency of binder,
Material costs can be reduced. Also, the addition of the binder increases the liquid content of the fleece and makes the fleece easy to handle, eliminating the need for a step of adjusting the liquid content in the fiber by adding oil for adjusting the liquid content, etc. The process can be simplified. Therefore, it is possible to increase the production efficiency and reduce the production cost. (2) Since hexamethylenetetramine, which easily generates gases such as formaldehyde and ammonia when heated, is not used as a curing agent, a bad odor caused by the curing agent during manufacturing or the curing agent is heated during the molding process. Thus, generation of smoke can be prevented, and deterioration of the working environment can be prevented. Further, the odor caused by the curing agent is prevented from remaining in the product, and the odor of the product can be suppressed. For this reason, even when the product is used as an interior material of an automobile, for example, where the odor stays in the closed space and is likely to cause a problem, for example, the product can be prevented from causing discomfort to the user. (3) By using a resol-type phenol resin binder having a property of being cured by heating as a liquid binder, a curing agent is not required, material costs can be reduced, and an odor caused by the curing agent can be prevented.
Also, the free formaldehyde content is low (for example, 0.5
By using a resol-type phenolic resin binder, the amount of formaldehyde emission from the product can be kept low, and the user can be prevented from feeling uncomfortable or deteriorating their health.
【0015】上記方法により得られたフェルトは、自動
車の内装材の他、家具類、家電類などの内装材、断熱
材、吸音材、緩衝材等として使用することができる。The felt obtained by the above method can be used as interior materials for automobiles, interior materials for furniture and home appliances, heat insulating materials, sound absorbing materials, cushioning materials and the like.
【0016】なお、上記方法では、液状バインダとし
て、フェノールとホルムアルデヒドを反応させることに
より得られた液状物、および上記反応により得られた固
形物の分散液を例示したが、これに限らず、フェノール
に代えて、クレゾール、レゾルシノール、3,5−キシ
レノール、ビスフェノールA、ビスフェノールF、その
他の置換フェノールなどのフェノール類化合物、または
これらの混合物を用いて得られたフェノール樹脂を含む
ものを用いることができる。また、ホルムアルデヒドに
代えて、アセトアルデヒド、パラホルムアルデヒド、ホ
ルマリン、ベンズアルデヒド、サリチルアルデヒド、フ
ルフラール、p−ヒドロキシベンズアルデヒド、テレフ
タルアルデヒド、またはこれらの混合物などのアルデヒ
ド類化合物を用いることもできる。この場合にも、液状
バインダの遊離フェノール類化合物含有量を5重量%未
満とし、遊離アルデヒド類化合物含有量を0.5重量%
未満とするのが好ましい。また、液状バインダには、必
要に応じて離型剤、潤滑剤、着色剤、難燃剤などの添加
剤を含有させることもできる。またこれらの添加剤は、
バインダに混合せず、バインダとは別に基材繊維に添加
してもよい。In the above method, a liquid material obtained by reacting phenol with formaldehyde and a dispersion liquid of a solid material obtained by the above reaction are exemplified as the liquid binder. Alternatively, phenolic compounds such as cresol, resorcinol, 3,5-xylenol, bisphenol A, bisphenol F, and other substituted phenols, or those containing a phenolic resin obtained using a mixture thereof can be used. . Also, instead of formaldehyde, aldehyde compounds such as acetaldehyde, paraformaldehyde, formalin, benzaldehyde, salicylaldehyde, furfural, p-hydroxybenzaldehyde, terephthalaldehyde, or a mixture thereof can be used. Also in this case, the content of the free phenol compound in the liquid binder is less than 5% by weight, and the content of the free aldehyde compound is 0.5% by weight.
It is preferred to be less than. Further, the liquid binder may contain additives such as a release agent, a lubricant, a coloring agent, and a flame retardant, if necessary. These additives also
Instead of being mixed with the binder, it may be added to the base fiber separately from the binder.
【0017】上記難燃剤としては、例えばトリフェニル
ホスフェート、トリクレジルホスフェート、クレジルフ
ェニルホスフェート、トリス(ハロプロピル)ホスフェ
ート、トリス(ハロエチル)ホスフェート等のリン酸エ
ステル系難燃剤、塩素化パラフィン、塩素化ポリエチレ
ン、パークロロペンタシクロデカン、ヘキサブロモベン
ゼン、デカブロモシフェニルエーテル、テトラブロモビ
スフェノールAおよびその誘導体、ヘキサブロモシクロ
ドデカンなどの含ハロゲン有機化合物、三酸化アンチモ
ン、アンチモン酸塩、メタホウ酸バリウム、ホウ酸亜
鉛、水酸化アルミニウム、アンモニウムブロマイド、硫
酸カルシウム水和物などの無機系難燃剤、テトラブロモ
無水フタル酸、ブロモスチレン、ビニルブロマイドなど
の反応型難燃剤が用いられ、リン系難燃剤、ハロゲン系
難燃剤がなかでも好ましい。また、ポリリン酸カルバメ
ートを使用してもよい。FMVSS−302(米国自動
車内装用品の安全規格Federal Motor VehicleSafety St
andard No.302)において不燃判定を得るためには、例
えばノンネンW−2−50(丸菱油化K.K.)を基材
繊維100重量部に対し2〜15重量部添加するのが好
ましい。またUL94(米国Standard for Tests for F
lammability of Plastic Materials for Parts in Devi
ces and Appliances -Forth Edition 1991)の94V−
0に合格するためには、例えば上記難燃剤(ノンネンW
−2−50)を基材繊維100重量部に対し15〜30
重量部添加するのが好ましい。Examples of the flame retardant include phosphoric ester flame retardants such as triphenyl phosphate, tricresyl phosphate, cresyl phenyl phosphate, tris (halopropyl) phosphate and tris (haloethyl) phosphate, chlorinated paraffin, and chlorine. Polyethylene, perchloropentacyclodecane, hexabromobenzene, decabromocyphenyl ether, tetrabromobisphenol A and its derivatives, halogen-containing organic compounds such as hexabromocyclododecane, antimony trioxide, antimonate, barium metaborate, Uses inorganic flame retardants such as zinc borate, aluminum hydroxide, ammonium bromide, calcium sulfate hydrate, and reactive flame retardants such as tetrabromophthalic anhydride, bromostyrene, and vinyl bromide It is, phosphorus-based flame retardant, a halogen-based flame retardant which preferable. Further, a polyphosphate carbamate may be used. FMVSS-302 (Federal Motor Vehicle Safetyty St.
andard No. 302), it is preferable to add, for example, 2 to 15 parts by weight of nonene W-2-50 (Marubishi Yuka KK) to 100 parts by weight of the base fiber in order to obtain a nonflammability determination. . UL94 (US Standard for Tests for F
lammability of Plastic Materials for Parts in Devi
ces and Appliances -Forth Edition 1991) 94V-
In order to pass 0, for example, the above-mentioned flame retardant (nonnene W
-2-50) is 15 to 30 with respect to 100 parts by weight of the base fiber.
It is preferable to add parts by weight.
【0018】[0018]
【実施例】以下、具体例を示して本発明の効果を明確に
する。 (実施例1)コットンまたはレーヨンを70〜80重量
%、合成繊維を20〜30重量%含む端切れを基材繊維
として用い、この基材繊維を細断後、液状バインダをス
プレー(噴出口径1.5mm)を用いて基材繊維に添
加、混合した。液状バインダとしては、レゾール型フェ
ノール樹脂液体バインダ(昭和高分子製ショウノールB
RL−192)を使用した。この液状バインダの遊離フ
ェノール含有量は3.8重量%、遊離ホルムアルデヒド
含有量は0.3重量%であった。液状バインダの添加量
は、基材繊維100重量部に対し15重量部とした。上
記基材繊維と液状バインダの混合物を、フリースマシン
を用いて解繊し、フリースを得た。これら混合物および
フリースのビニル袋詰め品内のフェノールおよびホルム
アルデヒドの気中濃度を、光明理化学K.K.製検知管
No.183U、およびNo.171SBを用いて測定
した結果、フェノールの気中濃度が0.3ppm未満、
ホルムアルデヒドの気中濃度が0.5ppm未満であ
り、いずれも十分に低い値となったことがわかった。次
に、得られたフリースをフォーミングし、プレス装置に
より230℃、663g/m2の条件下で3分間の加熱
成形を施し、長さ20cm、幅20cm、厚さ1.0c
mの矩形シート状のマットフェルト製品を得た。EXAMPLES The effects of the present invention will be clarified by showing specific examples. (Example 1) Cut pieces containing 70 to 80% by weight of cotton or rayon and 20 to 30% by weight of synthetic fibers were used as base fibers, and after chopping the base fibers, a liquid binder was sprayed (spout diameter 1. 5 mm) to the base fiber. As a liquid binder, a resol-type phenol resin liquid binder (Showa Polymer Shonor B)
RL-192). The liquid binder had a free phenol content of 3.8% by weight and a free formaldehyde content of 0.3% by weight. The added amount of the liquid binder was 15 parts by weight based on 100 parts by weight of the base fiber. The mixture of the base fiber and the liquid binder was defibrated using a fleece machine to obtain a fleece. The aerial concentrations of phenol and formaldehyde in the vinyl bag of these mixtures and fleece were determined by the method of Komei Rika K.K. K. Detector tube No. 183U, and no. As a result of measurement using 171SB, the air concentration of phenol was less than 0.3 ppm,
It was found that the aerial concentration of formaldehyde was less than 0.5 ppm, and all were sufficiently low values. Next, the obtained fleece is formed and subjected to heat molding for 3 minutes at 230 ° C. and 663 g / m 2 by a press device to obtain a length of 20 cm, a width of 20 cm, and a thickness of 1.0 c.
m was obtained in the form of a sheet-like mat felt product.
【0019】得られたマットフェルト製品を、以下に示
す各試験に供した。 (1)臭気試験 上記フェルト製品を長さ5cm、幅5cmの矩形状に裁
断した試験片を温度22℃、湿度60%の環境下に3日
間放置した後、10人のパネラーに嗅がせ、その臭気の
強度を4段階(0:無臭、1:弱い、2:強い、3:非
常に強い)のいずれかに判定させ、その平均値を算出し
た。また、臭気の快不快度を4段階(0:非常に不快、
1:不快、2:快、3:非常に快)のいずれかに判定さ
せ、その平均値を算出した。 (2)発煙の有無 加熱成形時にフリースが発煙したかどうかを目視にて確
認した。 (3)ホルムアルデヒド放散量 上記試験片のホルムアルデヒド放散量を測定した。試験
方法は、JIS A5908 5.11に準拠した。 (4)引張強さ 上記フェルト製品を長さ20cm、幅2.5cmの矩形
状に裁断した試験片に200mm/分の速度で引張力を
加え、試験片断面積あたりの最大破断荷重を算出した。 (5)難燃性 FMVSS−302に準拠した。試験結果を表1に示
す。なお、表中マット、ボードとは、それぞれマットフ
ェルト製品、ボードフェルト製品を指す。The obtained mat felt product was subjected to the following tests. (1) Odor test A test piece obtained by cutting the felt product into a rectangular shape having a length of 5 cm and a width of 5 cm was left in an environment of a temperature of 22 ° C. and a humidity of 60% for 3 days, and then smelled by 10 panelists. The odor intensity was determined in one of four levels (0: odorless, 1: weak, 2: strong, 3: very strong), and the average value was calculated. In addition, the odor pleasure and discomfort levels were graded in four stages (0: very
1: unpleasant, 2: pleasant, 3: very pleasant), and the average value was calculated. (2) Presence or absence of smoke It was visually confirmed whether or not the fleece smoked during the heat molding. (3) Formaldehyde emission amount The formaldehyde emission amount of the test specimen was measured. The test method was based on JIS A5908 5.11. (4) Tensile Strength A tensile force was applied at a speed of 200 mm / min to a test piece obtained by cutting the felt product into a rectangular shape having a length of 20 cm and a width of 2.5 cm, and a maximum breaking load per test piece cross-sectional area was calculated. (5) Flame retardancy Based on FMVSS-302. Table 1 shows the test results. The mat and board in the table refer to a mat felt product and a board felt product, respectively.
【0020】(実施例2)実施例1と同様にして得られ
たフリースを、14日間放置し、さらに90℃下で一晩
放置した後に加熱成形すること以外は実施例1と同様に
してマットフェルト製品を得た。このマットフェルト製
品を上記試験(1)〜(5)に供した。結果を表1に併
せて示す。Example 2 A mat was obtained in the same manner as in Example 1 except that the fleece obtained in the same manner as in Example 1 was left for 14 days, left at 90 ° C. overnight, and then heat-molded. A felt product was obtained. This mat felt product was subjected to the tests (1) to (5). The results are shown in Table 1.
【0021】(実施例3)液状バインダに、難燃剤ノン
ネンW−2−50(丸菱油化K.K.)を基材繊維10
0重量部に対して5重量部添加したこと以外は実施例1
と同様にしてマットフェルト製品を得た。このマットフ
ェルト製品を上記試験(1)〜(5)に供した結果を表
1に併せて示す。(Example 3) Non-flammable agent Nonen W-2-50 (Marubishi Yuka KK) was used as the base fiber 10 in a liquid binder.
Example 1 except that 5 parts by weight was added to 0 parts by weight.
In the same manner as above, a mat felt product was obtained. The results of subjecting this mat felt product to the above tests (1) to (5) are also shown in Table 1.
【0022】(実施例4)液状バインダの添加量を、基
材繊維100重量部に対し30重量部とし、フォーミン
グ形成したマットを150℃、3分間加熱して表層を固
めた後、さらに230℃、25kg/cm2 の圧力で、
1015g/m2の条件下で1分間加熱成形を施して長
さ20cm、幅20cm、厚さ0.20cmの矩形状の
ボードフェルト製品を得た。なおその他の試験条件は実
施例1と同様とした。得られたボードフェルト製品を、
上記試験(1)〜(3)、および以下に示す試験(6)
に供した。 (6)曲げ強さ 試験方法は、JIS A 5908 5.6に準拠した。
結果を表1に併せて示す。Example 4 The amount of the liquid binder added was 30 parts by weight with respect to 100 parts by weight of the base fiber. The formed mat was heated at 150 ° C. for 3 minutes to solidify the surface layer, and then at 230 ° C. At a pressure of 25 kg / cm 2 ,
Heat molding was performed for 1 minute under the conditions of 1015 g / m 2 to obtain a rectangular board felt product having a length of 20 cm, a width of 20 cm and a thickness of 0.20 cm. The other test conditions were the same as in Example 1. The obtained board felt product,
The above tests (1) to (3) and the following test (6)
Was served. (6) Flexural strength The test method was based on JIS A 5908 5.6.
The results are shown in Table 1.
【0023】(実施例5)ノボラック型フェノール樹脂
(昭和高分子製ショウノールBRP594P)100重
量部と、アニオン系乳化剤を3重量部と、硬化剤として
熱反応型水溶性ポリウレタン樹脂(第一工業製薬製エラ
ストロンH−3)10重量部と、水20重量部とを均一
混合したものをバインダとして用いること以外は実施例
4と同様にしてボードフェルト製品を得た。この製品を
上記試験(1)〜(3)、(6)に供した。結果を表1
に併せて示す。(Example 5) 100 parts by weight of a novolak type phenol resin (Showanol BRP594P manufactured by Showa Polymer), 3 parts by weight of an anionic emulsifier, and a heat-reactive water-soluble polyurethane resin (Daiichi Kogyo Seiyaku Co., Ltd.) as a curing agent A board felt product was obtained in the same manner as in Example 4 except that 10 parts by weight of Elastron H-3) and 20 parts by weight of water were uniformly mixed and used as a binder. This product was subjected to the tests (1) to (3) and (6). Table 1 shows the results
Are shown together.
【0024】(比較例1)実施例1に用いたものと同様
の基材繊維を細断後、解繊し、得られたフリースに、粉
末状のノボラック型フェノール樹脂とヘキサメチレンテ
トラミンとを混合して得たバインダ(昭和高分子製ショ
ウノールBRP5417、ノボラック型フェノール樹脂
とヘキサメチレンテトラミンの混合比100:10(重
量比))を添加、混合した。バインダの添加量は、フリ
ース100重量部に対し15重量部とした。次に、上記
フリースとバインダの混合物に、実施例1と同様の条件
で加熱成形を施し、長さ20cm、幅20cm、厚さ
1.0cmの矩形シート状のマットフェルト製品を得
た。このマットフェルト製品を上記試験(1)〜(5)
に供した。結果を表1に併せて示す。(Comparative Example 1) A base fiber similar to that used in Example 1 was cut and defibrated, and the obtained fleece was mixed with a powdery novolak type phenol resin and hexamethylenetetramine. (Showa Polymer's Shaunol BRP5417, a mixing ratio of novolak-type phenol resin and hexamethylenetetramine of 100: 10 (weight ratio)) was added and mixed. The amount of the binder was 15 parts by weight with respect to 100 parts by weight of the fleece. Next, the mixture of the fleece and the binder was subjected to heat molding under the same conditions as in Example 1 to obtain a rectangular sheet mat felt product having a length of 20 cm, a width of 20 cm, and a thickness of 1.0 cm. This mat felt product is subjected to the above tests (1) to (5)
Was served. The results are shown in Table 1.
【0025】(比較例2)バインダの添加量を、フリー
ス100重量部に対し10重量部とすること以外は比較
例1と同様にしてマットフェルト製品を得た。このマッ
トフェルト製品を上記試験(1)〜(5)に供した。結
果を表1に併せて示す。Comparative Example 2 A mat felt product was obtained in the same manner as in Comparative Example 1 except that the amount of the binder was 10 parts by weight with respect to 100 parts by weight of the fleece. This mat felt product was subjected to the tests (1) to (5). The results are shown in Table 1.
【0026】(比較例3)実施例1に用いたものと同様
の基材繊維を細断後、解繊し、得られたフリースに、バ
インダとして比較例1で用いたものと同じ昭和高分子製
ショウノールBRP5417を添加、混合した。バイン
ダの添加量は、フリース100重量部に対し35重量部
とした。次に、上記フリースとバインダの混合物に、実
施例4と同様の条件で加熱成形を施し、長さ20cm、
幅20cm、厚さ0.2cmの矩形シート状のボードフ
ェルト製品を得た。このボードフェルト製品を上記試験
(1)〜(3)、(6)に供した。結果を表1に併せて
示す。Comparative Example 3 The same base fiber as that used in Example 1 was shredded and defibrated, and the obtained fleece was used as a binder in the same Showa high polymer as that used in Comparative example 1. Shownol BRP5417 manufactured by the company was added and mixed. The amount of the binder was 35 parts by weight based on 100 parts by weight of the fleece. Next, the mixture of the fleece and the binder was subjected to heat molding under the same conditions as in Example 4 to have a length of 20 cm.
A rectangular sheet-shaped board felt product having a width of 20 cm and a thickness of 0.2 cm was obtained. This board felt product was subjected to the tests (1) to (3) and (6). The results are shown in Table 1.
【0027】(比較例4)バインダの添加量を、フリー
ス100重量部に対し30重量部とすること以外は比較
例3と同様にしてボードフェルト製品を得た。このボー
ドフェルト製品を上記試験(1)〜(3)、(6)に供
した。結果を表1に併せて示す。Comparative Example 4 A board felt product was obtained in the same manner as in Comparative Example 3 except that the amount of the binder was 30 parts by weight with respect to 100 parts by weight of the fleece. This board felt product was subjected to the tests (1) to (3) and (6). The results are shown in Table 1.
【0028】[0028]
【表1】 [Table 1]
【0029】表1より、バインダとしてノボラック型フ
ェノール樹脂とヘキサメチレンテトラミンの混合物を用
いた比較例では、得られた製品の臭気が比較的強くかつ
不快であり、ホルムアルデヒド放散量が多く、しかも製
造時に発煙が見られたのに対し、バインダとして液状バ
インダを用いた実施例では、製品の臭気が比較的弱くか
つ不快でなく、ホルムアルデヒド放散量が少なく、しか
も発煙が見られなかったことがわかる。From Table 1, it can be seen that in the comparative example using a mixture of novolak type phenol resin and hexamethylenetetramine as the binder, the obtained product has a relatively strong and unpleasant odor, a large amount of formaldehyde emission, and a large amount of formaldehyde emission. While smoke was observed, in the example using the liquid binder as the binder, it was found that the odor of the product was relatively weak and unpleasant, the amount of formaldehyde emission was small, and smoke was not observed.
【0030】[0030]
【発明の効果】本発明のフェルトの製造方法にあって
は、以下に示す効果を得ることができる。 (1)バインダが液状であるため、バインダが粉塵とな
って飛散することがなく、作業環境を良好に保つことが
できる。 (2)製造時において、硬化剤としてヘキサメチレンテ
トラミンを使用する必要がないため、この硬化剤を原因
とする悪臭や煙が発生するのを防ぐことができ、作業環
境の悪化を防ぐことができる。また、この硬化剤を原因
とする臭気が製品に残るのを防ぎ、利用者に不快感を与
えるのを防ぐことができる。According to the felt manufacturing method of the present invention, the following effects can be obtained. (1) Since the binder is in a liquid state, the binder is not scattered as dust, so that a favorable working environment can be maintained. (2) Since it is not necessary to use hexamethylenetetramine as a curing agent at the time of production, it is possible to prevent the generation of offensive odor and smoke caused by the curing agent and to prevent the working environment from deteriorating. . Further, it is possible to prevent the odor caused by the curing agent from remaining in the product, and to prevent the user from feeling uncomfortable.
───────────────────────────────────────────────────── フロントページの続き (72)発明者 岩田 立男 静岡県浜松市中沢町10番1号 ヤマハ株式 会社内 Fターム(参考) 4J002 AB01W AB01X AF02X AH00W BA01X BB12W BD04X BD10X BE06W BF02X BG00X CC04X CC16X CC18X CD00X CF00X CF03W CK02X CL00W CL00X CM04X DA016 DL006 FA04W FA046 GL00 GN00 GQ00 4L047 AA08 AA12 AA28 BA15 BC14 CB03 CB06 CC09 CC16 ────────────────────────────────────────────────── ─── Continuing on the front page (72) Tatsuo Iwata Inventor 10-1 Nakazawa-cho, Hamamatsu-shi, Shizuoka F-term in Yamaha Corporation (reference) 4J002 AB01W AB01X AF02X AH00W BA01X BB12W BD04X BD10X BE06W BF02X BG00X CC04X CC16X CC18X CD00X CF00X CF03W CK02X CL00W CL00X CM04X DA016 DL006 FA04W FA046 GL00 GN00 GQ00 4L047 AA08 AA12 AA28 BA15 BC14 CB03 CB06 CC09 CC16
Claims (5)
ースとし、このフリースを加熱成形することを特徴とす
るフェルトの製造方法。1. A method for manufacturing a felt, comprising adding a liquid binder to a base fiber to form a fleece, and heat-forming the fleece.
いて、液状バインダとして、フェノール樹脂を含むもの
を用いることを特徴とするフェルトの製造方法。2. The felt manufacturing method according to claim 1, wherein a liquid binder containing a phenol resin is used.
いて、フェノール樹脂としてレゾール型フェノール樹脂
を用いることを特徴とするフェルトの製造方法。3. The felt manufacturing method according to claim 2, wherein a resol type phenol resin is used as the phenol resin.
フェルトの製造方法によって得られたものであることを
特徴とするフェルト。4. A felt obtained by the method for producing a felt according to claim 1.
フェルトの製造方法に用いられるフェルト用バインダで
あって、液状物であることを特徴とするフェルト用バイ
ンダ。5. A felt binder used in the felt manufacturing method according to claim 1, wherein the felt binder is a liquid material.