CN1327545C - 用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶 - Google Patents

用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶 Download PDF

Info

Publication number
CN1327545C
CN1327545C CNB2004100772037A CN200410077203A CN1327545C CN 1327545 C CN1327545 C CN 1327545C CN B2004100772037 A CNB2004100772037 A CN B2004100772037A CN 200410077203 A CN200410077203 A CN 200410077203A CN 1327545 C CN1327545 C CN 1327545C
Authority
CN
China
Prior art keywords
acetone
polytetrafluoroethylene
epoxy resin
binding glue
lithium battery
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CNB2004100772037A
Other languages
English (en)
Other versions
CN1786097A (zh
Inventor
袁月馨
傅舒顺
刘聚龙
王继生
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shenzhen B & K Rechargeable Battery Inc.
Original Assignee
INTERSIL TECHNOLOGY (SHENZHEN) Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by INTERSIL TECHNOLOGY (SHENZHEN) Co Ltd filed Critical INTERSIL TECHNOLOGY (SHENZHEN) Co Ltd
Priority to CNB2004100772037A priority Critical patent/CN1327545C/zh
Publication of CN1786097A publication Critical patent/CN1786097A/zh
Application granted granted Critical
Publication of CN1327545C publication Critical patent/CN1327545C/zh
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

本发明涉及用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶,该粘接胶由丙酮、聚四氟乙烯以及环氧树脂制成的,其中各原料组份的重量百分比含量为,丙酮78-90%,聚四氟乙烯3-15%,环氧树脂3-12%。本隔膜粘接胶具有用量少、价格低廉、制作工艺简单及使用方便优点,并且能快速地把隔膜融合,使外层隔膜固定处平整,无厚度差,且不与电池内部其他化学物质发生化学反应等特点,粘接效果好,能够广泛地用于液态软包装或聚合物锂电池。

Description

用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶
技术领域
本发明涉及粘接胶技术,具体是一种用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶。
背景技术
近年来,液态软包装或聚合物锂电池的应用范围越来越广,市场对其质量要求也越来越严格。传统的电芯卷绕一般采用胶纸固定末端隔膜或极片,也有隔膜、极片末端不固定等。采用胶纸固定,由于胶纸本身具有一定厚度,所以导致电池外观不平整,电池厚度不均等,另外,引入胶纸容易导致电池内阻大、自放电大。如果隔膜或极片末端不固定,则会影响电芯的松紧程度,在抽真空封焊时,容易把隔膜纸或极片吸走偏位,从而影响电池外观及电池性能。
发明内容
为避免现有技术存在的上述不足,本发明提供一种使用方便、粘接效果好的液态软包装锂电池或聚合物锂电池的隔膜粘接胶。
本发明用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶是由丙酮、聚四氟乙烯以及环氧树脂制成的,其中各原料组份的重量百分比含量为,丙酮78-90%,聚四氟乙烯3-15%,环氧树脂3-12%。
本发明的隔膜粘接胶具有用量少、价格低廉、制作工艺简单及使用方便优点,并且能快速地把隔膜融合,使外层隔膜固定处平整,无厚度差,且不与电池内部其他化学物质发生化学反应等特点,粘接效果好,能够广泛地用于液态软包装或聚合物锂电池。
具体实施方式
以下结合实施例对本发明详细说明。
本发明液态软包装或聚合物锂电池隔膜粘接胶主要由丙酮、聚四氟乙烯以及环氧树脂制成,其中各原料组份的重量百分比含量为,丙酮78-90%,聚四氟乙烯3-15%,环氧树脂3-12%。使用时,将隔膜粘接胶直接涂擦在隔膜接口处即可进行快速融合。
实施例1:
取丙酮、聚四氟乙烯以及环氧树脂,按以下重量比丙酮∶聚四氟乙烯∶环氧树脂=85∶5∶10进行配料,其中丙酮做溶剂,聚四氟乙烯和环氧树脂为溶质,将聚四氟乙烯和环氧树脂直接加入丙酮中,搅拌均匀,待溶质溶解后过滤得透明溶液即为隔膜粘接胶。
实施例2:各原料组份按重量比丙酮∶聚四氟乙烯∶环氧树脂=80∶15∶5进行配料,丙酮做溶剂,聚四氟乙烯和环氧树脂做溶质,将溶质直接加入丙酮中,搅拌均匀,待溶质溶解后过滤得透明溶液即可。
本发明液态软包装或聚合物锂电池隔膜粘接胶可由丙酮、聚四氟乙烯、环氧树脂以及聚丙烯制成,各原料组份的重量百分比含量为:丙酮78-90%,聚四氟乙烯3-15%,环氧树脂3-12%,聚丙烯2-5%。
实施例3:
各原料组份按重量比丙酮∶聚四氟乙烯∶环氧树脂∶聚丙烯=80∶10∶5∶5进行配料,丙酮做溶剂,将溶质聚四氟乙烯、环氧树脂及聚丙烯直接加入丙酮中,搅拌均匀,待溶质溶解后过滤得透明溶液即可。
实施例4:
按重量比丙酮∶聚四氟乙烯∶环氧树脂∶聚丙烯=88∶4∶6∶2进行配料,将聚四氟乙烯、环氧树脂及聚丙烯直接加入丙酮中,搅拌均匀,待溶解后过滤得透明溶液即可。
本液态软包装或聚合物锂电池隔膜粘接胶可由丙酮、聚四氟乙烯、环氧树脂以及聚乙烯制成,其中各原料组份的重量百分比含量为,丙酮78-90%,聚四氟乙烯3-15%,环氧树脂3-12%,聚乙烯2-5%。
实施例5:
按重量比丙酮∶聚四氟乙烯∶环氧树脂∶聚乙烯=80∶10∶7∶3进行配料,丙酮做溶剂,其余做溶质,将所有溶质直接加入丙酮中,搅拌均匀,待溶质溶解后过滤得透明溶液即可。
实施例6:
按重量比丙酮∶聚四氟乙烯∶环氧树脂∶聚乙烯=85∶6∶5∶4配料,丙酮做溶剂,其余做溶质,将所有溶质直接加入丙酮中,搅拌均匀,待溶质溶解后过滤得透明溶液即可。
本液态软包装或聚合物锂电池隔膜粘接胶也可采用78-90%的丙酮、3-15%的聚四氟乙烯、3-12%的环氧树脂、2-5%的聚丙烯,2-5%的聚乙烯混合、溶解制成。
实施例7:
按重量比丙酮∶聚四氟乙烯∶环氧树脂∶聚丙烯∶聚乙烯=85∶3∶5∶3∶4进行配料,丙酮做溶剂,其余做溶质,将所有溶质直接加入丙酮中,搅拌均匀,待溶质溶解后过滤得透明溶液即可。
实施例8:
按重量比丙酮∶聚四氟乙烯∶环氧树脂∶聚丙烯∶聚乙烯=78∶8∶8∶4∶2进行配料,丙酮做溶剂,其余做溶质,将所有溶质直接加入丙酮中,搅拌均匀,待溶质溶解后过滤得透明溶液即可。

Claims (4)

1、一种用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶,其特征是:该隔膜粘接胶是由丙酮、聚四氟乙烯以及环氧树脂制成的,其中各原料组份的重量百分比含量为,丙酮78-90%,聚四氟乙烯3-15%,环氧树脂3-12%。
2、根据权利要求1所述的用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶,其特征是:该隔膜粘接胶还含有聚丙烯,聚丙烯的重量百分比含量为2-5%。
3、根据权利要求1所述的用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶,其特征是:该隔膜粘接胶还含有聚乙烯,聚乙烯的重量百分比含量为2-5%。
4、根据权利要求1所述的用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶,其特征是:该隔膜粘接胶还含有聚丙烯和聚乙烯,聚丙烯的重量百分比含量为2-5%,聚乙烯的重量百分比含量为2-5%。
CNB2004100772037A 2004-12-09 2004-12-09 用于制造软包装锂电池或聚合物锂电池的隔膜粘接胶 Expired - Fee Related CN1327545C (zh)