[go: up one dir, main page]

CN115491491B - 一种冶金炉混合熔剂配料方法 - Google Patents

一种冶金炉混合熔剂配料方法 Download PDF

Info

Publication number
CN115491491B
CN115491491B CN202211092010.3A CN202211092010A CN115491491B CN 115491491 B CN115491491 B CN 115491491B CN 202211092010 A CN202211092010 A CN 202211092010A CN 115491491 B CN115491491 B CN 115491491B
Authority
CN
China
Prior art keywords
soot
rotary kiln
converter
furnace
precious metal
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN202211092010.3A
Other languages
English (en)
Other versions
CN115491491A (zh
Inventor
秦海燕
李育平
陈文斌
李睿
雷国强
郑广明
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jinchuan Group Copper Precious Metals Co.,Ltd.
Original Assignee
Jinchuan Group Co Ltd
Jinchuan Group Copper Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jinchuan Group Co Ltd, Jinchuan Group Copper Co Ltd filed Critical Jinchuan Group Co Ltd
Priority to CN202211092010.3A priority Critical patent/CN115491491B/zh
Publication of CN115491491A publication Critical patent/CN115491491A/zh
Application granted granted Critical
Publication of CN115491491B publication Critical patent/CN115491491B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种冶金炉混合熔剂配料方法,该方法是指将转炉余热炉烟灰、回转窑烧结物、转炉一周期冷料、回转窑烟灰、电炉烟灰按任意比例混合均匀后得到杂料;然后在所述杂料中依次加入贵金属冶炼分银渣、石英石,混合后进入立式磨研磨系统,即得粒度‑60目>90%且SiO2含量为75%~85%的混合熔剂。本发明简单、安全,解决了生产难题和被动局面,提升了产能,增加了经济效益。

Description

一种冶金炉混合熔剂配料方法
技术领域
本发明涉及冶金工艺领域,尤其涉及一种冶金炉混合熔剂配料方法。
背景技术
冶金炉熔炼所需熔剂(SiO2)的主要作用是与氧化反应生成的Fe3O4、熔锍中的FeS以及碱性氧化物等进行造渣反应。冶金炉应用单喷咀技术,炉内熔炼反应强度、深度得到优化,小时投料量显著提升,实现了自热熔炼。但炉内热量过剩成为制约处理量进一步提升的主要因素,严重威胁炉体安全。此外在冶炼过程中产生的低热中间物料大量堆积,重复加工、拉运,造成能耗成本增加。
发明内容
本发明所要解决的技术问题是提供一种简单、安全的冶金炉混合熔剂配料方法。
为解决上述问题,本发明所述的一种冶金炉混合熔剂配料方法,其特征在于:该方法是指将转炉余热炉烟灰、回转窑烧结物、转炉一周期冷料、回转窑烟灰、电炉烟灰按任意比例混合均匀后得到杂料;然后在所述杂料中依次加入贵金属冶炼分银渣、石英石,混合后进入立式磨研磨系统,即得粒度-60目>90%且SiO2含量为75%~85%的混合熔剂;所述贵金属冶炼分银渣与所述杂料的质量比为1:2;所述石英石与所述贵金属冶炼分银渣+杂料之和的质量比为9:1。
所述转炉余热炉烟灰中含Cu 48.92%,含S 10.156%。
所述回转窑烧结物中含Cu 24.54%,含S 11.24%。
所述转炉一周期冷料中含Cu 20.28%,含S 13.54%。
所述回转窑烟灰或所述电炉烟灰中含Cu 17~18%,含S 10~11%。
所述贵金属冶炼分银渣中含S 3.79%;石英石SiO含量95%以上。
本发明与现有技术相比具有以下优点:
1、本发明中转炉余热炉烟灰、回转窑烧结物、转炉一周期冷料、回转窑烟灰、电炉烟灰、贵金属冶炼分银渣作为低热物料与石英石进行混合配料,使得低热物料在内部循环利用,不仅为冶金炉补充了必需的低热物料,保证了冶金炉的高负荷安全稳定生产;而且避免了中间物料重复加工、拉运的环节,解决了物料大量积存的问题。
2、本发明采用低热物料混合配料方式,最终达到了降低炉内热量,消除炉体安全隐患的目的,不但方法简单,而且提升了产能,增加了经济效益。
具体实施方式
一种冶金炉混合熔剂配料方法,该方法是指将转炉余热炉烟灰、回转窑烧结物、转炉一周期冷料、回转窑烟灰、电炉烟灰按任意比例混合均匀后得到杂料;然后在杂料中依次加入贵金属冶炼分银渣、石英石,混合后进入立式磨研磨系统,即得粒度-60目>90%且SiO2含量为75%~85%的混合熔剂。所得混合熔剂作为平衡冶金炉(闪速炉)热负荷的原料之一再加入到冶金炉内进行造渣反应。
其中:贵金属冶炼分银渣与杂料的质量比(kg/kg)为1:2。
石英石与贵金属冶炼分银渣+杂料之和的质量比(kg/kg)为9:1。
转炉余热炉烟灰中含Cu 48.92%,含S 10.156%。
回转窑烧结物中含Cu 24.54%,含S 11.24%。
转炉一周期冷料中含Cu 20.28%,含S 13.54%。
回转窑烟灰或电炉烟灰中含Cu 17~18%,含S 10~11%。
贵金属冶炼分银渣中含S 3.79%;石英石SiO含量95%以上。
本发明中转炉余热炉烟灰与熔剂(石英石)的混合配料,既解决了冶金炉(闪速炉)所需的低热物料,又避免了回转窑烧结物进入原流程处理过程产生的电能消耗。
本发明中回转窑烧结物、转炉一周期冷料与熔剂(石英石)的混合配料,既解决了冶金炉(闪速炉)所需的低热物料,又提高了冶炼回收率,同时解决了物流不平衡带来的生产管理和组织困难。
本发明中回转窑烟灰、电炉烟灰与熔剂(石英石)的混合配料,既解决了冶金炉(闪速炉)所需的低热物料,又避免了回转窑烟灰、电炉烟灰进入原流程处理过程产生的电能消耗。
本发明中贵金属冶炼分银渣与熔剂(石英石)的混合配料,既解决了冶金炉(闪速炉)所需的低热物料,又回收该物料中的有价金属,同时解决了物料积压的问题。
实施例 一种冶金炉混合熔剂配料方法,该方法是指将0.2t/h转炉余热炉烟灰、0.2t/h回转窑烧结物、0.4t/h转炉一周期冷料、0.4t/h 回转窑烟灰、0.4t/h电炉烟灰混合均匀后得到杂料;然后在杂料中依次加入0.8t/h贵金属冶炼分银渣、21.6t/h石英石,混合后进入立式磨研磨系统,即得24t/h粒度-60目>90%且SiO2含量为75~85%的混合熔剂。
各低热物料成份见表1~表6。
表1 转炉余热炉烟灰成份
表2 回转窑烧结物成份
表3 转炉一周期冷料成份
表4 回转窑烟灰成份
表5 电炉烟灰成份
表6 贵金属分银渣成份

Claims (1)

1.一种冶金炉混合熔剂配料方法,其特征在于:该方法是指将转炉余热炉烟灰、回转窑烧结物、转炉一周期冷料、回转窑烟灰、电炉烟灰按任意比例混合均匀后得到杂料;然后在所述杂料中依次加入贵金属冶炼分银渣、石英石,混合后进入立式磨研磨系统,即得粒度-60目>90%且SiO2含量为75%~85%的混合熔剂;所述贵金属冶炼分银渣与所述杂料的质量比为1:2;所述石英石与所述贵金属冶炼分银渣+杂料之和的质量比为9:1;所述转炉余热炉烟灰中含Cu 48.92%,含S 10.156%;所述回转窑烧结物中含Cu 24.54%,含S 11.24%;所述转炉一周期冷料中含Cu 20.28%,含S 13.54%;所述回转窑烟灰或所述电炉烟灰中含Cu 17~18%,含S 10~11%;所述贵金属冶炼分银渣中含S 3.79%;石英石SiO含量95%以上。
CN202211092010.3A 2022-09-07 2022-09-07 一种冶金炉混合熔剂配料方法 Active CN115491491B (zh)