CN106365171A - Quickly-drying silicon sol and preparation method thereof - Google Patents

Quickly-drying silicon sol and preparation method thereof Download PDF

Info

Publication number
CN106365171A
CN106365171A CN201610730102.8A CN201610730102A CN106365171A CN 106365171 A CN106365171 A CN 106365171A CN 201610730102 A CN201610730102 A CN 201610730102A CN 106365171 A CN106365171 A CN 106365171A
Authority
CN
China
Prior art keywords
ludox
humic acid
preparation
quick
dried
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201610730102.8A
Other languages
Chinese (zh)
Other versions
CN106365171B (en
Inventor
闫森源
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Strong New Genuine (suzhou) Environmental Mstar Technology Ltd
Original Assignee
Strong New Genuine (suzhou) Environmental Mstar Technology Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Strong New Genuine (suzhou) Environmental Mstar Technology Ltd filed Critical Strong New Genuine (suzhou) Environmental Mstar Technology Ltd
Priority to CN201610730102.8A priority Critical patent/CN106365171B/en
Publication of CN106365171A publication Critical patent/CN106365171A/en
Application granted granted Critical
Publication of CN106365171B publication Critical patent/CN106365171B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a preparation method of quickly-drying silicon sol. The preparation method includes the steps of: S01) preparing a humic acid solution and regulating the pH thereof to 8-10; S02) dropwise adding the humic acid solution to a silicon sol solution, and stirring and mixing the mixture to form a humic acid/silicon sol mixture system; S03) filtering the humic acid/silicon sol mixture system and washing the mixture system with anhydrous ethanol, and re-dispersing the filtered mixture in a polyamide latex water solution to prepare the quickly-drying silicon sol. In the quickly-drying silicon sol, SiO2 particles are uniformly dispersed in the polymer emulsion. The product is cost-saving and is environment-protective.

Description

A kind of dry quick Ludox and preparation method thereof
Technical field
The present invention relates to a kind of be dried quick Ludox and preparation method thereof, belong to technical field of nano material.
Background technology
Ludox is dispersion liquid in water or in solvent for the nano level silica dioxide granule, has specific surface area big, resistance to The characteristics such as high temperature, antioxidation, are that a kind of preferable polymer emulsion increases
Strong material.Due to nanometer sio in Ludox2There is great amount of hydroxy group in particle surface, need to carry out hydrophobically modified to it, make sio2Particle can be uniformly dispersed in polymer emulsion.So far, main modifying agent mainly includes machine modifying agent and gold Belong to modifying agent two big class.Organic modifiers are mainly silane coupler, but silane coupler can occur violent water in water Solution condensation reaction, leads to the generation of gel;What metal modifiers were commonly used is aluminum, stannum, zinc and lead, but the cost of metal modifiers Higher, the problems such as in addition can cause heavy metal pollution.In addition, common Ludox slow drying speed, the production cycle is caused to extend, It is unfavorable for the raising of production efficiency.
Content of the invention
The technical problem to be solved in the present invention is to provide that a kind of Ludox arid cycle is short, sio2Uniform particle is scattered The preparation method of quick Ludox is dried;Further, the present invention provides a kind of quick silicon of cost-effective, environment-friendly type drying molten Glue and preparation method thereof.
For solving above-mentioned technical problem, the technical solution used in the present invention is:
A kind of dry quick Ludox preparation method, comprises the following steps:
S01, prepares Humic Acid Solution, and then carry out acid-alkali accommodation to make its ph is between 8 ~ 10;
S02, the Humic Acid Solution obtaining in s01 is added drop-wise to stirring mixing in silicon sol solution, forms humic acid/Ludox and mixes Fit system;
S03, with dehydrated alcohol is washed after the humic acid obtaining/Ludox mixed system is filtered in s02, finally will The mixture being filtrated to get is re-dispersed in polyamide emulsion hydrosol, is obtained and quick Ludox is dried.
The concentration of described silicon sol solution is 30 ~ 40wt%.
Described humic acid extracts from the soil organism or water body organic matter.
The acid of described acid-alkali accommodation includes dilute hydrochloric acid or dust technology, and the alkali of described acid-alkali accommodation includes sodium hydroxide.
The concentration of described humic acid is between 1000mg/l to 2000mg/l.
Any one of following condition or multinomial is also included in s02:
A. the reaction temperature of described stirring mixing is 40oC to 50oBetween c;
B. described stirring is mixed into continuously stirred mixing, and the time of described continuously stirred mixing is at least 24 hours;
C. the drop rate of described humic acid is 5 ~ 10ml/min.
A kind of dry quick Ludox, is obtained by aforementioned preparation process.
Beneficial effects of the present invention: a kind of rapid draing Ludox that the present invention provides and preparation method thereof, polyamide breast The setting of glue, can shorten Ludox arid cycle, and the Humic Acid Solution obtaining in s01 is added drop-wise to stirring in silicon sol solution Mixing, forms humic acid/Ludox mixed system, sio2Particle can adsorb the humic acid with negative charge so as to itself carries There is negative charge, increase sio2Repulsive interaction between particle, final sio2Particle in water or in solvent dispersed formation be difficult The Ludox stability reunite, generating is high;Described humic acid extracts from the soil organism or water body organic matter, and humic acid exists It is widely present in nature, occupies the major part in natural organic matter, from humic acid as the material of modified silicasol, become This is relatively low, and humic acid itself is extremely stable, generation environment will not pollute, has the effect of environmental protection.
Specific embodiment
The knot present invention is further described below, and following examples are only used for the technical side of the present invention is clearly described Case, and can not be limited the scope of the invention with this.
Embodiment 1
A kind of dry quick Ludox preparation method, comprises the following steps:
S01, prepares Humic Acid Solution, and then carry out acid-alkali accommodation to make its ph is 8;
S02, the Humic Acid Solution obtaining in s01 is added drop-wise to stirring mixing in silicon sol solution, forms humic acid/Ludox and mixes Fit system;
S03, with dehydrated alcohol is washed after the humic acid obtaining/Ludox mixed system is filtered in s02, finally will The mixture being filtrated to get is re-dispersed in polyamide emulsion hydrosol, is obtained and quick Ludox is dried.
The concentration of described silicon sol solution is 30wt%.
Described humic acid extracts from the soil organism or water body organic matter.
The acid of described acid-alkali accommodation includes dilute hydrochloric acid or dust technology, and the alkali of described acid-alkali accommodation includes sodium hydroxide.
The concentration of described humic acid is 1000mg/l.
Any one of following condition or multinomial is also included in s02:
A. the reaction temperature of described stirring mixing is 40oc;
B. described stirring is mixed into continuously stirred mixing, at least 24 hours time of described continuously stirred mixing;
C. the drop rate of described humic acid is 5ml/min.
A kind of dry quick Ludox, is obtained by aforementioned preparation process.
Embodiment 2
A kind of dry quick Ludox preparation method, comprises the following steps:
S01, prepares Humic Acid Solution, and then carry out acid-alkali accommodation to make its ph is 10;
S02, the Humic Acid Solution obtaining in s01 is added drop-wise to stirring mixing in silicon sol solution, forms humic acid/Ludox and mixes Fit system;
S03, with dehydrated alcohol is washed after the humic acid obtaining/Ludox mixed system is filtered in s02, finally will The mixture being filtrated to get is re-dispersed in polyamide emulsion hydrosol, is obtained and quick Ludox is dried.
The concentration of described silicon sol solution is 40wt%.
Described humic acid extracts from the soil organism or water body organic matter.
The acid of described acid-alkali accommodation includes dilute hydrochloric acid or dust technology, and the alkali of described acid-alkali accommodation includes sodium hydroxide.
The concentration of described humic acid is 2000mg/l.
Any one of following condition or multinomial is also included in s02:
A. the reaction temperature of described stirring mixing is 50oc;
B. described stirring is mixed into continuously stirred mixing, at least 24 hours time of described continuously stirred mixing;
C. the drop rate of described humic acid is 10ml/min.
A kind of dry quick Ludox, is obtained by aforementioned preparation process.
The above be only the preferred embodiment of the present invention it should be pointed out that: for the ordinary skill people of the art For member, under the premise without departing from the principles of the invention, some improvements and modifications can also be made, these improvements and modifications also should It is considered as protection scope of the present invention.

Claims (7)

1. a kind of quick Ludox preparation method is dried it is characterised in that: comprise the following steps:
S01, prepares Humic Acid Solution, and then carry out acid-alkali accommodation to make its ph is between 8 ~ 10;
S02, the Humic Acid Solution obtaining in s01 is added drop-wise to stirring mixing in silicon sol solution, forms humic acid/Ludox and mixes Fit system;
S03, with dehydrated alcohol is washed after the humic acid obtaining/Ludox mixed system is filtered in s02, finally will The mixture being filtrated to get is re-dispersed in polyamide emulsion hydrosol, is obtained and quick Ludox is dried.
2. according to claim 1 a kind of quick Ludox preparation method is dried it is characterised in that: described silicon sol solution Concentration be 30 ~ 40wt%.
3. according to claim 1 a kind of quick Ludox preparation method is dried it is characterised in that: described humic acid is from soil Extract in earth organic matter or water body organic matter.
4. according to claim 1 a kind of quick Ludox preparation method is dried it is characterised in that: described acid-alkali accommodation Acid includes dilute hydrochloric acid or dust technology, and the alkali of described acid-alkali accommodation includes sodium hydroxide.
5. according to claim 1 a kind of quick Ludox preparation method is dried it is characterised in that: described humic acid dense Spend between 1000mg/l to 2000mg/l.
6. a kind of preparation method that quick Ludox is dried according to claim 1 is it is characterised in that also wrap in s02 Include any one of following condition or multinomial:
A. the reaction temperature of described stirring mixing is 40oC to 50oBetween c;
B. described stirring is mixed into continuously stirred mixing, and the time of described continuously stirred mixing is at least 24 hours;
C. the drop rate of described humic acid is 5 ~ 10ml/min.
7. a kind of quick Ludox is dried it is characterised in that: any one of claim 1-6, preparation method is obtained.
CN201610730102.8A 2016-08-26 2016-08-26 A kind of quick Ludox of drying and preparation method thereof Active CN106365171B (en)