CN106273048A - A kind of preparation method of antioxidation master batch - Google Patents
A kind of preparation method of antioxidation master batch Download PDFInfo
- Publication number
- CN106273048A CN106273048A CN201610645467.0A CN201610645467A CN106273048A CN 106273048 A CN106273048 A CN 106273048A CN 201610645467 A CN201610645467 A CN 201610645467A CN 106273048 A CN106273048 A CN 106273048A
- Authority
- CN
- China
- Prior art keywords
- master batch
- antioxidation
- preparation
- screw extruder
- double screw
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The present invention provides the preparation method of a kind of antioxidation master batch, comprises the following steps: the first step, mixing: raw material age resistor TMQ, antioxidant 2112 and antioxidant AO 60 are stirred by the weight ratio of 3:2:5 successively;Second step, banburying: by the premix material feeding double screw extruder prepared in the first step or single screw extrusion machine, first preheating 35 minutes, wherein each district temperature of double screw extruder is 185 230 DEG C, and the rotating speed of double screw extruder is 250 500 revs/min;3rd step, pelletize: in second step, the material of extrusion is cut through air-cooled flour milling and is drawn into master batch;4th step, is dehydrated and packs, and by the master batch made in the 3rd step dehydration and packs in time.The antioxidation master batch stable chemical performance that the present invention produces, antioxygenic property is good, and effect is lasting, and cost of manufacture is relatively low.
Description
Technical field
The invention belongs to plastic and manufacture field, particularly relate to the preparation method of a kind of antioxidation master batch.
Background technology
Plastic master batch i.e. plastic matrix, is that plastic additive super quantity is attached to the condensation product made in resin;System
When making plastic, it is not necessary to add this kind of plastic additive, and only need to add corresponding masterbatch, thus, it is to work as this life
One of main form of boundary's plastic additive application.Its advantage is: technique is simple, easy to use, it is simple to realize the production automation,
Raise labour productivity, avoid again the cleaning of environmental pollution, beneficially workers ' health to carry out production strictly in line with rules and regulations, and plastics preparation, processing,
Storage and during using, easily occur oxidation reaction and presenting to fade, yellowing, the phenomenon of cracking, its hot strength and impact are strong
The mechanical performances such as degree reduce, and most plastic not UV radiation, it is impossible to life-time service out of doors, therefore female
The antioxygenic property of grain directly affects the quality of plastic.
Summary of the invention
In view of this, it is contemplated that propose a kind of preparation method with good antioxygenic property master batch.
For reaching above-mentioned purpose, the technical scheme is that and be achieved in that: the preparation method of a kind of antioxidation master batch,
Comprise the following steps: the first step, mixing: raw material age resistor TMQ, antioxidant 2112 and antioxidant AO-60 are pressed 3:2:5's successively
Ratio carries out high-speed mixer stirring;
Second step, banburying: by the premix material feeding double screw extruder prepared in the first step or single screw extrusion machine, first
Preheating 3-5 minute, wherein each district temperature of double screw extruder is 185-230 DEG C, and the rotating speed of double screw extruder is 250-
500 revs/min;
3rd step, pelletize: in second step, the material of extrusion is cut through air-cooled flour milling and is drawn into master batch;
4th step, is dehydrated and packs.
Further, use high-speed mixer stirring, at temperature 60-80 DEG C, carry out mixed at high speed 3-5 minute, described mixed
The rotating speed of conjunction machine is 1000-2000 rev/min.
Further, also including processing aid in raw material, the total content of processing aid is 3-5wt%.
Further, the draw ratio of described single screw extrusion machine is 20-55, and the control temperature of operation is Solid Conveying and Melting respectively
District is 130-140 DEG C, 160-170 DEG C of material plasticizing district, 170-180 DEG C, melt delivery area, described single screw extrusion machine rotating speed is
300-1000 rev/min.
Further, employing aluminium foil bag encapsulation is packed described in.
The present invention has the advantage that with good effect: compared with prior art, 1, the present invention uses internally mix to add extrusion and make
Grain continuous print production technology, it efficiently solves in production process and easily builds bridge, and disperses uneven problem;2, the present invention's is anti-
Oxidation master batch can be greatly promoted the antioxygenic property of plastics, effectively promotes service life and the performance of plastics;3, possesses antioxidation
Function, effect is lasting, and has preferable stability, and cost of manufacture is relatively low.
Detailed description of the invention
It should be noted that in the case of not conflicting, the embodiment in the invention and the feature in embodiment can
To be mutually combined.
Below the specific embodiment of the present invention is elaborated.
Embodiment 1: the preparation method of a kind of antioxidation master batch, the first step, mixing: by raw material age resistor TMQ, antioxidant
2112 and antioxidant AO-60 carry out high-speed mixer stirring in the ratio of 3:2:5 successively, it is possible to additionally incorporate the processing aid of 3wt%,
Carrying out mixed at high speed under temperature 60 C 3 minutes, the rotating speed of described mixer is 1000 revs/min;Second step, banburying: by first
The premix material feeding double screw extruder prepared in step, first preheats 3 minutes, and wherein each district temperature of double screw extruder is
185 DEG C, the rotating speed of double screw extruder is 250 revs/min;3rd step, pelletize, in second step, the material of extrusion is again through air-cooled flour milling
Cut and be drawn into master batch;4th step, is dehydrated and packs.
Embodiment 2: the preparation method of a kind of antioxidation master batch, the first step, mixing: by raw material age resistor TMQ, antioxidant
2112 and antioxidant AO-60 carry out high-speed mixer stirring in the ratio of 3:2:5 successively, it is possible to additionally incorporate the processing aid of 4wt%,
Carrying out mixed at high speed under temperature 70 C 4 minutes, the rotating speed of described mixer is 1500 revs/min;Second step, banburying: by first
The premix material feeding double screw extruder prepared in step, first preheats 4 minutes, and wherein each district temperature of double screw extruder is
200 DEG C, the rotating speed of double screw extruder is 380 revs/min;3rd step, pelletize, in second step, the material of extrusion is again through air-cooled flour milling
Cut and be drawn into master batch;4th step, is dehydrated and packs.
Embodiment 3: the preparation method of a kind of antioxidation master batch, the first step, mixing: by raw material age resistor TMQ, antioxidant
2112 and antioxidant AO-60 carry out high-speed mixer stirring in the ratio of 3:2:5 successively, it is possible to additionally incorporate the processing aid of 5wt%,
Carrying out mixed at high speed 5 minutes at temperature 80 DEG C, the rotating speed of described mixer is 2000 revs/min;Second step, banburying: by first
The premix material feeding double screw extruder prepared in step, first preheats 5 minutes, and wherein each district temperature of double screw extruder is
230 DEG C, the rotating speed of double screw extruder is 500 revs/min;3rd step, pelletize, in second step, the material of extrusion is again through air-cooled flour milling
Cut and be drawn into master batch;4th step, is dehydrated and packs.
Note also problems with in the above process, each steps flow chart is held in strict accordance with the temperature and time set
OK, it is ensured that each processing step operation preparatory, it is ensured that the quality of volume production master batch, so ensure plastic product performance.
Above one embodiment of the present of invention is described in detail, but described content has been only the preferable enforcement of the present invention
Example, it is impossible to be considered the practical range for limiting the present invention.All impartial changes made according to the present patent application scope and improvement
Deng, within all should still belonging to the patent covering scope of the present invention.
Claims (5)
1. the preparation method of an antioxidation master batch, it is characterised in that: comprise the following steps:
The first step, mixing: raw material age resistor TMQ, antioxidant 2112 and antioxidant AO-60 are adopted by the weight ratio of 3:2:5 successively
Stir with high-speed mixer;
Second step, banburying: the premix material prepared in the first step is fed in double screw extruder or single screw extrusion machine, first pre-add
Hot 3-5 minute, wherein each district temperature of double screw extruder was 185-230 DEG C, and the rotating speed of double screw extruder is 250-500
Rev/min;
3rd step, pelletize: in second step, the material of extrusion is cut through air-cooled flour milling and is drawn into master batch;
4th step, is dehydrated and packs.
The preparation method of a kind of antioxidation master batch the most according to claim 1, it is characterised in that: use described mixed at high speed
Machine, carries out mixed at high speed 3-5 minute at temperature 60-80 DEG C, and the rotating speed of described mixer is 1000-2000 rev/min.
The preparation method of a kind of antioxidation master batch the most according to claim 1, it is characterised in that: raw material also includes processing
Auxiliary agent, the total content of processing aid is 3-5wt%.
The preparation method of a kind of antioxidation master batch the most according to claim 1, it is characterised in that: described single screw extrusion machine
Draw ratio be 20-55, the control temperature of operation be respectively solid conveying zone be 130-140 DEG C, material plasticizing district 160-170
DEG C, 170-180 DEG C, melt delivery area, described single screw extrusion machine rotating speed is 300-1000 rev/min.
The preparation method of a kind of antioxidation master batch the most according to claim 1, it is characterised in that pack employing described in:
Aluminium foil bag encapsulates.