CN106245415A - A kind of manufacture method of glassine paper - Google Patents
A kind of manufacture method of glassine paper Download PDFInfo
- Publication number
- CN106245415A CN106245415A CN201610725022.3A CN201610725022A CN106245415A CN 106245415 A CN106245415 A CN 106245415A CN 201610725022 A CN201610725022 A CN 201610725022A CN 106245415 A CN106245415 A CN 106245415A
- Authority
- CN
- China
- Prior art keywords
- paper
- pulp
- applying glue
- slurry
- page
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention discloses the manufacture method of a kind of glassine paper, including use softwood pulp, hardwood pulp through making beating respectively, with slurry and adjuvant adds, l Water Paper page is manufactured paper with pulp, front be dried, coating applying glue (PVA), the rear processing step such as dry.The present invention, by studying the functionalized chemical auxiliary agent etc. added in slurry selection, wet end furnish, beating process, slurry, uses film transitional surface applying glue to process, and performs to produce qualified glassine paper with reference to relevant paper machine parameter.
Description
Technical field
The present invention relates to the manufacture method of a kind of glassine paper, belong to pulp technology for making paper.
Background technology
Glassine paper is a kind of industrial paper, makes Ge Laxin after the operations such as rewetting, supercalendering and painting silicone oil
Paper.Lattice Racine paper (GLASSINE) quality is fine and close, uniform, has good internal intensity and transparency.Be make bar coded sticker,
Adhesive sticker, adhesive tape or the common used material of toughness industrial goods.The functions such as lattice Racine paper has certain high temperature resistant, moistureproof, grease proofing,
It is generally used for the packaging of the industry such as food, medicine.It is mainly used in: High-Speed Automatic labeling (particularly suitable high speed label stickup) is special
Adhesive tape, two-sided tape base material trade mark, laser anti-counterfeit mark and other release application etc..Medical product is mainly used for as glue
Band and the release paper of casting product.Conventional grammes per square metre is 58g-120g.The purposes of lattice Racine paper and top grade two-sided film release paper
Similar, owing to this product is more environmentally-friendly, the market share from now on will be increasing.Domestic so that the people live in plenty in Zhejiang special paper, Zhejiang five
It is main that the enterprises such as continent paper industry, justice south, Yiwu paper industry, Wuhan Chenming's paper industry produce Ge Laxin (former) paper, along with the change of market capacity
Greatly, increasing enterprise by participation exploitation and produces Ge Laxin (former) paper.My company is not because having supercalender, therefore only
Develop glassine paper.
Glassine paper is processed as Ge Laxin paper process: body paper rewetting--supercalendering---being coated with silicone oil---rewind slitting
Lattice Racine paper primary quality measure includes: smoothness, transparency, water absorption, tensile strength, homogeneity etc..
The glassine paper of my company's exploitation in 2016, main innovation point has: (i) from slurry selection, beating process and papermaking
Technical study and innovation, the product quality at the glassine paper of PM9 exploitation fully meets the use requirement of client, mainly studies
Including: 1. study grout structure;Selecting commodity sulfate bleached wood pulp (needle and broad-leaved) is primary raw material.2. research is optimal
Wet end furnish;By laboratory handsheet and the research with slurry of paper machine, determine optimal wet end furnish scope----softwood pulp: leaf wood
Slurry=(70-80): (30-20).3. optimal beating degree span of control is studied, in order to allow paper machine be dehydrated and manufacture paper with pulp normal, with
Time meet and improve needle slurry ratio, it is ensured that end product Ge Laxin paper transparency is high;We start with research from beating process, pass through
Use fast beating mode test of many times research, overturned general Ge Laxin paper beating process, finally determined optimal
Beating degree span of control is (as broad-leaved slurry beating degree controls 22-260SR, needle slurry beating degree controls 22-300SR).4. use
Film transitional surface sizing equipment carries out top sizing process, and glassine paper does not use Oxytarch glue-applying technique, but adopts
With the glue-applying technique of full PVA, boil technique and insulation is operated after all being groped by many experiments and just determines, it is ensured that the PVA of ton paper
Resin added reaches 15-20kg.(ii) product structure innovation transition, (call of response company, product is tied to promote company's profitability
Structure is made the transition to industry paper by Cultural Paper, and glassine paper rate of gross profit is apparently higher than company's existing product);Simultaneously market share by
Year increases, and is an industrial paper new product being worth exploitation.
Summary of the invention
It is an object of the invention to provide the manufacture method of a kind of glassine paper.
The technical scheme is that the manufacture method of a kind of glassine paper, including using softwood pulp, leaf wood
Slurry, through making beating respectively, with slurry and adjuvant adds, l Water Paper page is manufactured paper with pulp, front be dried, coating applying glue, after the processing step such as be dried, it is special
Levy and be:
(1) sulfate wood pulp slurry weight proportioning, softwood pulp: hardwood pulp=70-80: 30-20;
(2) freedom after slurry pulping: softwood pulp 22-30 SR;Hardwood pulp 22-26 SR;
(3) oven dry stock consumption is by adjuvant: (a) AKD weight ratio 1.5-2.0%;(b) retention agent weight ratio 0.02-
0.04%;(c) cationic starch weight ratio 0.8-1.0%;
(4) applying glue portion: with PVA, boil concentration 9%, upper gum concentration 4.0%, it is ensured that PVA coating weight is at 15-20kg/ ton paper.Metering
Rod type number: 1#, gauge stick pressure 100kpa;Up/down roller applying glue flow is respectively 1050L/min/1050L/min;Surface, two sides
Applying glue, one side controls at 0.5-0.8g/m2, page tension force 220N/m before applying glue portion2, page tension force 200N/m behind applying glue portion2;
(5) other parameters of paper machine: network speed 680m/min, push up net dehydrating amount 27%, head box opening degree of slice lip 9.7mm, a line ball
Pressure: 900 kN/m, two line ball pressure: 900 kN/m;Curl tension: 400kN/m;
(6) rolling condition: calender separately, is not pressurized;
(7) glassine paper is quantitative: 62-78g/m2, moisture (4.0-7.0%), form and aspect raw white, longitudinal fracture length (>=
7.0Km), water absorption (20-28g/m2), tightness (≤0.74g/m2), air permeability (≤120ml/min), transversal stretching rate (≤
3.0%), thickness is stable, formation of sheet good, planarization is good.
The present invention is by grinding the functionalized chemical auxiliary agent etc. added in slurry selection, wet end furnish, beating process, slurry
Study carefully, use film transitional surface applying glue to process, perform to produce qualified glassine paper, to company with reference to relevant paper machine parameter
Optimize product structure and to promote company's profitability significant.
Detailed description of the invention
Embodiment 1:78 gram glassine paper
By softwood pulp, (beating degree controls at 22-260SR) and hardwood pulp (beating degree controls at 22-260SR) two kinds of slurries
Material carries out with slurry in the ratio of 70%:30%, add 15-20kg/ ton paper AKD sizing agent, add in 8-10kg/ ton paper pulp sun from
Sub-starch, addition 0.2-0.4kg/ ton paper retention agent, be configured to the approach flow that raw white has diluted, carry out two-sided by folded net
Dehydration, it is ensured that fiber is uniformly dispersed, vertically and horizontally fiber alignment is orderly and is uniformly distributed, after l Water Paper page enters press section unipress;
Being dried the page entrance applying glue portion to mass dryness fraction 95% before entering, (surface is executed to use film branch mode that paper is carried out top sizing process
Glue sizing material is mainly composed of PVA);The control total resin added of PVA is at 15-20kg/ ton paper, and l Water Paper page after treatment is dry after entering
Dry process;After dried later, the mass dryness fraction page in 94~95% passes through soft press-polishing machine (calender up-down rollers is separately), then
Paper is batched, i.e. can get quantification of 78 g/m2Glassine paper, its leading indicator: moisture (4.0-7.0%),
Form and aspect raw white, longitudinal fracture length (>=7.0Km), water absorption (20-28g/m2), tightness (≤0.74g/m2), air permeability (≤
120ml/min), transversal stretching rate (≤3.0%), thickness is stable, formation of sheet good, planarization is good.Permissible according to process above
Produce qualified glassine paper, the prescription of client can be met completely.
Embodiment 2:62 gram glassine paper
By softwood pulp, (beating degree controls at 26-300SR) and hardwood pulp (beating degree controls at 22-260SR) two kinds of slurries
Material carries out with slurry in the ratio of 80%:20%, add 15-20kg/ ton paper AKD sizing agent, add in 8-10kg/ ton paper pulp sun from
Sub-starch, addition 0.2-0.4kg/ ton paper retention agent, be configured to the approach flow that raw white has diluted, carry out two-sided by folded net
Dehydration, it is ensured that fiber is uniformly dispersed, vertically and horizontally fiber alignment is orderly and is uniformly distributed, after l Water Paper page enters press section unipress;
Being dried the page entrance applying glue portion to mass dryness fraction 95% before entering, (surface is executed to use film branch mode that paper is carried out top sizing process
Glue sizing material is mainly composed of PVA);The control total resin added of PVA is at 15-20kg/ ton paper, and l Water Paper page after treatment is dry after entering
Dry process;After dried later, the mass dryness fraction page in 94~95% passes through soft press-polishing machine (calender up-down rollers is separately), then
Paper is batched, i.e. can get quantification of 62 g/m2Glassine paper, its leading indicator: moisture (4.0-7.0%),
Form and aspect raw white, longitudinal fracture length (>=7.0Km), water absorption (20-28g/m2), tightness (≤0.74g/m2), air permeability (≤
120ml/min), transversal stretching rate (≤3.0%), thickness is stable, formation of sheet good, planarization is good.Permissible according to process above
Produce qualified glassine paper, the prescription of client can be met completely.
Claims (1)
1. a manufacture method for glassine paper, including use softwood pulp, hardwood pulp, through respectively making beating, with slurry and auxiliary
Material adds, l Water Paper page is manufactured paper with pulp, front dry, coating applying glue, rear drying process step, it is characterised in that:
(1) sulfate wood pulp slurry weight proportioning, softwood pulp: hardwood pulp=70-80: 30-20;
(2) freedom after slurry pulping: softwood pulp 22-30 SR;Hardwood pulp 22-26 SR;
(3) oven dry stock consumption is by adjuvant: (a) AKD weight ratio 1.5-2.0%;(b) retention agent weight ratio 0.02-
0.04%;(c) cationic starch weight ratio 0.8-1.0%;
(4) applying glue portion: with PVA, boil concentration 9%, upper gum concentration 4.0%, it is ensured that PVA coating weight is at 15-20kg/ ton paper.Metering
Rod type number: 1#, gauge stick pressure 100kpa;Up/down roller applying glue flow is respectively 1050L/min/1050L/min;Surface, two sides
Applying glue, one side controls at 0.5-0.8g/m2, page tension force 220N/m before applying glue portion2, page tension force 200N/m behind applying glue portion2;
(5) other parameters of paper machine: network speed 680m/min, push up net dehydrating amount 27%, head box opening degree of slice lip 9.7mm, a line ball
Pressure: 900 kN/m, two line ball pressure: 900 kN/m;Curl tension: 400kN/m;
(6) rolling condition: calender separately, is not pressurized;
(7) glassine paper is quantitative: 62-78g/m2, moisture 4.0-7.0%, form and aspect raw white, longitudinal fracture length >=7.0Km,
Water absorption 20-28g/m2, tightness≤0.75g/m2, air permeability≤120ml/min, transversal stretching rate≤3.0%, thickness is stable, paper
Evenness is good, planarization is good.