CN105463643A CN201510805698.9A CN201510805698A CN105463643A CN 105463643 A CN105463643 A CN 105463643A CN 201510805698 A CN201510805698 A CN 201510805698A CN 105463643 A CN105463643 A CN 105463643A
Authority
CN
China
Prior art keywords
cotton fiber
fiber
hours
reeling
cotton
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN201510805698.9A
Other languages
Chinese (zh)
Inventor
陆卫新
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
CHANGSHU DREAM DEAN FURNISHINGS PRODUCTS Co Ltd
Original Assignee
CHANGSHU DREAM DEAN FURNISHINGS PRODUCTS Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by CHANGSHU DREAM DEAN FURNISHINGS PRODUCTS Co Ltd filed Critical CHANGSHU DREAM DEAN FURNISHINGS PRODUCTS Co Ltd
Priority to CN201510805698.9A priority Critical patent/CN105463643A/en
Publication of CN105463643A publication Critical patent/CN105463643A/en
Withdrawn legal-status Critical Current

Links

Classifications

    • DTEXTILES; PAPER
    • D02YARNS; MECHANICAL FINISHING OF YARNS OR ROPES; WARPING OR BEAMING
    • D02GCRIMPING OR CURLING FIBRES, FILAMENTS, THREADS, OR YARNS; YARNS OR THREADS
    • D02G3/00Yarns or threads, e.g. fancy yarns; Processes or apparatus for the production thereof, not otherwise provided for
    • D02G3/02Yarns or threads characterised by the material or by the materials from which they are made
    • D02G3/04Blended or other yarns or threads containing components made from different materials
    • DTEXTILES; PAPER
    • D02YARNS; MECHANICAL FINISHING OF YARNS OR ROPES; WARPING OR BEAMING
    • D02GCRIMPING OR CURLING FIBRES, FILAMENTS, THREADS, OR YARNS; YARNS OR THREADS
    • D02G3/00Yarns or threads, e.g. fancy yarns; Processes or apparatus for the production thereof, not otherwise provided for
    • D02G3/02Yarns or threads characterised by the material or by the materials from which they are made
    • D02G3/04Blended or other yarns or threads containing components made from different materials
    • D02G3/042Blended or other yarns or threads containing components made from different materials all components being made from natural material
    • DTEXTILES; PAPER
    • D06TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06BTREATING TEXTILE MATERIALS USING LIQUIDS, GASES OR VAPOURS
    • D06B3/00Passing of textile materials through liquids, gases or vapours to effect treatment, e.g. washing, dyeing, bleaching, sizing, impregnating
    • D06B3/04Passing of textile materials through liquids, gases or vapours to effect treatment, e.g. washing, dyeing, bleaching, sizing, impregnating of yarns, threads or filaments
    • DTEXTILES; PAPER
    • D06TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06BTREATING TEXTILE MATERIALS USING LIQUIDS, GASES OR VAPOURS
    • D06B9/00Solvent-treatment of textile materials

Landscapes

  • Engineering & Computer Science (AREA)
  • Textile Engineering (AREA)
  • Mechanical Engineering (AREA)
  • Coloring (AREA)

Abstract

The invention discloses a method producing cotton fiber colored spun yarns. The method comprises the following steps of conducting refining treatment to cotton fibers, (2) applying penetrant to cotton fibers, (3) winding yarns, (4) dying, (5) fixing color for two and a half hours at the temperature of 125 DEG C and (5) spinning, wherein in the (1) step, 5 to 7% of owf scouring agent is applied to the cotton fibers at the temperature of 65 DEG C and the cotton fibers are refined at a neutral condition for 3 to 5 hours; in the (2) step, 3 to 4g/L polyoxyethylene sorbitan fatty acid ester,2 to 3g/Llauryl sodium sulfate and 3 to 4 g/L polyvinylpyrrolidone are added; in the (3) step, the yarn winding weight is 550g; in the (4) step, dyestuff can be stripping dye or non-stripping dye; dying solution further contains 25g/L sodium bicarbonate during dying; and in the (6) step, cotton fibers of different colors can be interweaved into colored spinning yarns. By the use of the method, cotton fiber fabric with various colors and lasting color can be produced and color types of the cotton fiber fabric can be enriched.

Description

For the production of the method for cotton fiber fiber dyed yarn
Technical field
The present invention relates to the method for the production of cotton fiber fiber dyed yarn.
Background technology
Colour-spun yarns is the yarn be spun into by the fibers mixture of two or more different color and luster.Colour-spun yarns generally adopts the mode of dye cotton or sliver dyeing, contaminate color and be monochrome, the colour-spun yarns that spins all have colour mixture comparatively evenly, feature that cyclicity is strong, lack certain randomness and erratic behavior, can not meet consumer's craving for peculiar style.Tradition DISCHARGE PRINTING fabric is mainly weaved with gray yarn, then drift is boiled rear with dyeing can be pulled out, after dyeing, carry out DISCHARGE PRINTING again, most DISCHARGE PRINTING fabric is all adopt this processing method in the market, although meet the demand of printing and dyeing to a certain extent, dye after the change of its pattern is also confined to dawn, often contaminating a chromatography just increases cost again.
Summary of the invention
The object of the present invention is to provide a kind of method for the production of cotton fiber fiber dyed yarn, can shades of colour be produced and cotton fiber fabric not easy to fade, enrich the color variety of cotton fiber fabric.
For achieving the above object, technical scheme of the present invention is a kind of method for the production of cotton fiber fiber dyed yarn of design, comprises the steps:
1) cotton fiber refining process, 5-7%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 3-5 hour;
2) cotton fiber penetrant treating, adds 3-4g/L polyoxyethylene sorbitan fatty acid ester, 2-3g/L lauryl sodium sulfate, 3-4g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
Preferably, for the production of the method for cotton fiber fiber dyed yarn, comprise the steps:
1) cotton fiber refining process, 7%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 5 hours;
2) cotton fiber penetrant treating, adds 4g/L polyoxyethylene sorbitan fatty acid ester, 3g/L lauryl sodium sulfate, 4g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
Preferably, for the production of the method for cotton fiber fiber dyed yarn, comprise the steps:
1) cotton fiber refining process, 5%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 3 hours;
2) cotton fiber penetrant treating, adds 3g/L polyoxyethylene sorbitan fatty acid ester, 2g/L lauryl sodium sulfate, 3g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
Preferably, for the production of the method for cotton fiber fiber dyed yarn, comprise the steps:
1) cotton fiber refining process, 5.7%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 3.5 hours;
2) cotton fiber penetrant treating, adds 3.4g/L polyoxyethylene sorbitan fatty acid ester, 2.3g/L lauryl sodium sulfate, 3.4g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
Advantage of the present invention and beneficial effect are: provide a kind of method for the production of cotton fiber fiber dyed yarn, can produce shades of colour and cotton fiber fabric not easy to fade, enrich the color variety of cotton fiber fabric.
Detailed description of the invention
Below in conjunction with embodiment, the specific embodiment of the present invention is further described.Following examples only for technical scheme of the present invention is clearly described, and can not limit the scope of the invention with this.
The technical scheme that the present invention specifically implements is:
Embodiment 1
For the production of the method for cotton fiber fiber dyed yarn, comprise the steps:
1) cotton fiber refining process, 7%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 5 hours;
2) cotton fiber penetrant treating, adds 4g/L polyoxyethylene sorbitan fatty acid ester, 3g/L lauryl sodium sulfate, 4g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
Embodiment 2
For the production of the method for cotton fiber fiber dyed yarn, comprise the steps:
1) cotton fiber refining process, 5%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 3 hours;
2) cotton fiber penetrant treating, adds 3g/L polyoxyethylene sorbitan fatty acid ester, 2g/L lauryl sodium sulfate, 3g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
Embodiment 3
For the production of the method for cotton fiber fiber dyed yarn, comprise the steps:
1) cotton fiber refining process, 5.7%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 3.5 hours;
2) cotton fiber penetrant treating, adds 3.4g/L polyoxyethylene sorbitan fatty acid ester, 2.3g/L lauryl sodium sulfate, 3.4g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
The above is only the preferred embodiment of the present invention; it should be pointed out that for those skilled in the art, under the prerequisite not departing from the technology of the present invention principle; can also make some improvements and modifications, these improvements and modifications also should be considered as protection scope of the present invention.

Claims (4)

1. for the production of the method for cotton fiber fiber dyed yarn, it is characterized in that, comprise the steps:
1) cotton fiber refining process, 5-7%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 3-5 hour;
2) cotton fiber penetrant treating, adds 3-4g/L polyoxyethylene sorbitan fatty acid ester, 2-3g/L lauryl sodium sulfate, 3-4g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
2. the method for the production of cotton fiber fiber dyed yarn according to claim 1, is characterized in that, comprise the steps:
1) cotton fiber refining process, 7%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 5 hours;
2) cotton fiber penetrant treating, adds 4g/L polyoxyethylene sorbitan fatty acid ester, 3g/L lauryl sodium sulfate, 4g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
3. the method for the production of cotton fiber fiber dyed yarn according to claim 1, is characterized in that, comprise the steps:
1) cotton fiber refining process, 5%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 3 hours;
2) cotton fiber penetrant treating, adds 3g/L polyoxyethylene sorbitan fatty acid ester, 2g/L lauryl sodium sulfate, 3g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
4. the method for the production of cotton fiber fiber dyed yarn according to claim 1, is characterized in that, comprise the steps:
1) cotton fiber refining process, 5.7%owf scouring agent, at 65 DEG C, in neutral conditions, refining time is 3.5 hours;
2) cotton fiber penetrant treating, adds 3.4g/L polyoxyethylene sorbitan fatty acid ester, 2.3g/L lauryl sodium sulfate, 3.4g/L polyvinylpyrrolidone;
3) reeling: the weight of reeling is 550g;
4) dye, dyestuff be can discharge material or can not discharge material, also contains 25g/L sodium bicarbonate during dyeing in dye liquor used;
5) 125 DEG C of fixation 2.5 hours;
6) spin, the cotton fiber of different colours is woven into fiber dyed yarn.
CN201510805698.9A 2015-11-20 2015-11-20 Method producing cotton fiber colored spun yarns Withdrawn CN105463643A (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN201510805698.9A CN105463643A (en) 2015-11-20 2015-11-20 Method producing cotton fiber colored spun yarns

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN201510805698.9A CN105463643A (en) 2015-11-20 2015-11-20 Method producing cotton fiber colored spun yarns

Publications (1)

Publication Number Publication Date
CN105463643A true CN105463643A (en) 2016-04-06

Family

ID=55601780

Family Applications (1)

Application Number Title Priority Date Filing Date
CN201510805698.9A Withdrawn CN105463643A (en) 2015-11-20 2015-11-20 Method producing cotton fiber colored spun yarns

Country Status (1)

Country Link
CN (1) CN105463643A (en)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN108914292A (en) * 2018-08-01 2018-11-30 湖南莎丽袜业股份有限公司 A kind of number colour-spun yarns and its processing method, system and application

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN108914292A (en) * 2018-08-01 2018-11-30 湖南莎丽袜业股份有限公司 A kind of number colour-spun yarns and its processing method, system and application

Similar Documents

Publication Publication Date Title
CN100560858C (en) Discharge method of colored woven fabric and dischargeable colored spun yarn used therein
CN1865559B (en) Milk protein fiber or its filament or its blended fabric weaving and dyeing method
CN106939515B (en) The preparation of ball warp mercerization and efficient silkete penetrating agent in a kind of production of denim fabric
CN102154826B (en) Method for processing full real silk heterochromatic jacquard fabric
CN111188208A (en) Printing and dyeing process of cloth
CN105463878A (en) Dyeing or topping method for jeans yarns/garments
CN105019263A (en) Printing and dyeing agent for polyester-nylon-cotton blended fabric and printing and dyeing technology using the same
CN103147201B (en) A kind of production method of cotton fiber fiber dyed yarn
DE582101C (en) Process for improving the fastness properties of textiles dyed with water-soluble dyes
CN103015225A (en) Method for dyeing milk fiber and cotton blended fabric
CN110592979A (en) Nylon collagen fabric and dyeing and finishing method thereof
CN100422411C (en) Production for wool textile containing regenerating animal azelon
CN105463643A (en) Method producing cotton fiber colored spun yarns
CN108866705A (en) A kind of preparation process flow of long colored spun flax yarn
CN103215713B (en) Production method of bastose wet spinning yarn
CN102534902B (en) A kind of production method of two-color spun yarns
CN105063937A (en) Manufacturing method of jet dyed cashmere fancy yarns
CN112981646A (en) Method for manufacturing yak wool loop yarn
CN104074063A (en) Cationic fluorescent dyeing process for cotton fabrics
CN102704092B (en) A kind of iridescent yarn and production method thereof
CN102817131A (en) Cotton fiber dyed spun yarn and preparation method thereof
CN103215714A (en) Cotton and linen fiber colored spun yarn and manufacturing method thereof
CN110016816A (en) A kind of indigo dyeing method
CN109355938A (en) A kind of One Bath Dyeing of the wool blended fabric of spun silk
CN103952925B (en) A kind of cashmere bobbin dyeing technology

Legal Events

Date Code Title Description
C06 Publication
PB01 Publication
C10 Entry into substantive examination
SE01 Entry into force of request for substantive examination
WW01 Invention patent application withdrawn after publication
WW01 Invention patent application withdrawn after publication

Application publication date: 20160406