CN105127340B CN201510611318.8A CN201510611318A CN105127340B CN 105127340 B CN105127340 B CN 105127340B CN 201510611318 A CN201510611318 A CN 201510611318A CN 105127340 B CN105127340 B CN 105127340B
Authority
CN
China
Prior art keywords
rolling
ring
groove
blank
alpha
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201510611318.8A
Other languages
English (en)
Other versions
CN105127340A (zh
Inventor
秦芳诚
李永堂
刘志奇
齐会萍
李志�
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Taiyuan University of Science and Technology
Original Assignee
Taiyuan University of Science and Technology
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Taiyuan University of Science and Technology filed Critical Taiyuan University of Science and Technology
Priority to CN201510611318.8A priority Critical patent/CN105127340B/zh
Publication of CN105127340A publication Critical patent/CN105127340A/zh
Application granted granted Critical
Publication of CN105127340B publication Critical patent/CN105127340B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Links

Landscapes

  • Reduction Rolling/Reduction Stand/Operation Of Reduction Machine (AREA)
  • Metal Rolling (AREA)
  • Rolling Contact Bearings (AREA)

Abstract

一种凹槽斜内孔环件辗扩成形方法,属于环件辗扩成形技术领域,其特征在于工艺步骤如下:1)确定辗扩比λ;2)根据环件尺寸、辗扩比和体积不变原理,确定矩形截面毛坯尺寸,包括外径D0、内径d0和高度H0;3)辗扩孔型设计:根据毛坯和环件的尺寸结构及变形条件,设计驱动辊和芯辊的工作面型腔尺寸;4)确定辗扩工艺参数,包括驱动辊转速、芯辊进给速度、初始辗扩温度以及辗扩终了温度;5)辗扩成形:根据上述设计参数,在闭式辗环机上经连续多道次变形使环坯直径不断扩大、斜内孔和凹槽截面辗扩成形。本发明优点是凹槽斜内孔环件辗扩过程稳定,工艺参数设计合理,环件外形尺寸精确、性能质量好,辗环成品率高,能源和材料浪费低。

Description

一种凹槽斜内孔环件辗扩成形方法
技术领域
本发明属于环件辗扩成形技术领域,具体涉及一种凹槽斜内孔环件辗扩成形方法。
背景技术
凹槽环件是指外表面或内表面带有凹槽(槽深约占壁厚的五分之一以上)的异形环件,图1所示环件的凹槽深度占壁厚的二分之一,且内孔和凹槽上、下内壁具有一定的斜度,形状尺寸复杂。工程领域常用的双边支重轮体、混凝土搅拌车支撑导轨、双边法兰和高压球阀体等关键基础件均属于凹槽环件,对其尺寸精度、性能质量以及组织稳定性的要求较高。该类型环件的凹槽难以通过模锻直接成形,通常是先模锻简单预制坯成形,再经过机械切削加工出凹槽部位尺寸,但这会导致环件周向金属纤维流线在切削过程中被破坏,组织性能恶化,生产效率低、材料浪费严重。
发明内容
本发明的目的是提供一种凹槽斜内孔环件辗扩成形方法,可以有效地克服现有技术存在的缺点。
本发明的目的是这样实现的,其特征在于工艺步骤如下:如图1~5所示,
(1)确定辗扩比λ,即根据给定的环件形状尺寸按经验选取辗扩比的范围,λ=du/d0,其中du和d0分别为环件凹槽部位的内径和毛坯的内径,λ的取值范围为2.0~2.5;
(2)根据凹槽环件尺寸、辗扩比和辗扩变形前后体积不变原理,确定矩形截面环形毛坯尺寸,凹槽环件体积为:
其中,D为环件外径,d2为斜内孔小内径,H为轴向高度,h为凹槽外沿与环件上下端面之间尺寸,h1为凹槽外沿高度,Ru为凹槽圆弧半径,α1、α2为凹槽上、下内壁与水平面夹角,β为斜内孔壁与环件轴向夹角,辗扩变形前后轴向高度尺寸不变,即毛坯高度H0=H,毛坯内径d0=du/λ,毛坯外径
(3)辗扩孔型设计:根据毛坯和环件的尺寸结构、截面形状及辗扩变形条件,设计驱动辊和芯辊的工作面型腔尺寸;驱动辊为主轧辊,其工作面型腔与凹槽环件截面形状对应,芯辊工作面设计为中部带外台阶形状,辗扩变形过程采用闭式孔型,芯辊外台阶沿环坯径向不断将其压入驱动辊工作面型腔;驱动辊与芯辊的工作面半径应满足:(1/RM1+1/RI)≤1.75θ/H0,RM1为驱动辊最大型腔位置半径,RI为芯辊外台阶半径,θ=tan-1μ为摩擦角,μ为摩擦系数,取值范围为0.5~0.7,RM1、RI根据总进给量Δh=[(D0-d0)-(D-du)]/2并结合与辗扩过程咬入条件和锻透条件的关系确定;芯辊外台阶高度与驱动辊工作面型腔高度一致,工作面型腔高度HM=H0+6~10mm,且为了提高辗扩时金属的流动性,设计型腔上下内壁与水平面夹角γ为0°~6°;
(4)确定辗扩工艺参数,包括驱动辊转速、芯辊进给速度、初始辗扩温度以及辗扩终了温度:辗扩过程中驱动辊转速采用28.3~30.6r/min,芯辊进给速度采用不同的规范,咬入阶段进给速度由0mm/s增加到1.5mm/s,逐渐咬入形成凹槽轮廓,完成凹槽部位成形总量的30%;稳定辗扩阶段由1.5mm/s增加到2.0mm/s,快速辗扩得到凹槽完整形状,凹槽部位成形达到90%;精确校圆、整形阶段由2.0mm/s减小到0.5mm/s,对凹槽和斜内孔尺寸进行校整;根据锻造温度范围确定初始辗扩温度为1100~1150℃,并控制辗扩终了温度在870~900℃;
(5)辗扩成形:根据上述设计参数,在闭式辗环机上经过连续多道次变形使环坯直径不断扩大、斜内孔和凹槽截面辗扩成形。
本发明的优点及积极效果:采用本发明可以实现凹槽斜内孔环件辗扩过程的稳定进行和工艺参数的合理设计,环件的外形尺寸精确、内部组织性能质量较高,提高了辗环成品率,降低了能源和材料的浪费。
附图说明
图1为凹槽斜内孔环件的截面示意图。
图2为毛坯的截面示意图。
图3为驱动辊截面示意图。
图4为芯辊截面示意图。
图5为凹槽斜内孔环件辗扩示意图。
图中:1-芯辊 2-导向辊 3-凹槽斜内孔环件 4-驱动辊
D—环件外径,H—轴向高度,d1—斜内孔大内径,d2—斜内孔小内径,h—凹槽外沿与环件上下端面之间尺寸,h1—凹槽外沿高度,Ru—凹槽圆弧半径,du—凹槽部位内径,α1—凹槽上内壁与水平面夹角,α2—凹槽下内壁与水平面夹角,β—斜内孔壁与环件轴向夹角,D0—毛坯外径,H0—毛坯高度,d0—毛坯内径,DM—驱动辊外径,RM1—驱动辊最大型腔位置半径,DM1—驱动辊最大型腔位置直径,RI—芯辊外台阶半径,HM—工作面型腔高度,γ—型腔上下内壁与水平面夹角,DI—芯辊外台阶外径,HI—芯辊外台阶高度,dI—芯辊内台阶外径
具体实施方式
以图1所示凹槽斜内孔环件为具体实施例,要求辗扩成形的凹槽斜内孔环件尺寸为:环件外径D=1843mm,斜内孔大内径d1=1715mm,斜内孔小内径d2=1686mm,轴向高度H=60mm,凹槽圆弧半径Ru=12mm,凹槽部位内径du=1783mm,凹槽外沿与环件上下端面之间尺寸h=15mm,凹槽外沿高度h1=30mm,凹槽上、下内壁与水平面夹角α1、α2分别为6°、5°,斜内孔壁与环件轴向夹角β为14°;辗扩成形的工艺步骤是:如图1~5所示,
(1)确定辗扩比λ,根据给定的环件形状尺寸按经验选取辗扩比的范围,λ=du/d0,其中du和d0分别为环件凹槽部位的内径和毛坯的内径,该实施例取λ=2.2;
(2)根据凹槽环件尺寸、辗扩比和辗扩变形前后体积不变原理,确定矩形截面环形毛坯尺寸,凹槽环件体积为:
辗扩变形前后轴向高度尺寸不变,即毛坯高度H0=H=60mm,毛坯内径d0=du/λ=810mm,毛坯外径
(3)辗扩孔型设计:根据毛坯坯和环件的尺寸结构、截面形状及辗扩变形条件,设计驱动辊和芯辊的工作面型腔尺寸,驱动辊为主轧辊,其工作面型腔与凹槽环件截面形状对应,芯辊工作面设计为中部带外台阶形状,辗扩变形过程采用闭式孔型,芯辊外台阶沿环坯径向不断将其压入驱动辊工作面型腔;驱动辊与芯辊的工作面半径应满足:(1/RM1+1/RI)≤1.75θ/H0,RM1为驱动辊最大型腔位置半径,RI为芯辊外台阶半径,θ=tan-1μ为摩擦角,μ为摩擦系数,取μ=0.6,RM1、RI根据总进给量Δh=[(D0-d0)-(D-du)]/2并结合与辗扩过程咬入条件和锻透条件的关系确定,RM1=170mm,RI=220mm;芯辊外台阶高度与驱动辊工作面型腔高度一致,工作面型腔高度HM=H0+6~10mm=70mm,且为了提高辗扩时金属的流动性,设计型腔上下内壁与水平面夹角γ为0°~6°,该实例中取γ为5°;
(4)确定辗扩工艺参数,包括驱动辊转速、芯辊进给速度、初始辗扩温度以及辗扩终了温度:辗扩过程中驱动辊转速采用28.3r/min,芯辊进给速度采用不同的规范,咬入阶段进给速度由0mm/s增加到1.5mm/s,逐渐咬入形成凹槽轮廓,完成凹槽部位成形总量的30%;稳定辗扩阶段由1.5mm/s增加到2.0mm/s,快速辗扩得到凹槽完整形状,凹槽部位成形达到90%;精确较圆、整形阶段由2.0mm/s减小到0.5mm/s,对凹槽和斜内孔尺寸进行校整;根据锻造温度范围确定初始辗扩温度为1140℃,并控制辗扩终了温度在890℃;
(5)辗扩成形:根据上述设计参数,在闭式辗环机上经过连续多道次变形使环坯直径不断扩大、斜内孔和凹槽截面辗扩成形。

Claims (1)

1.一种凹槽斜内孔环件辗扩成形方法,其特征在于工艺步骤如下:
(1)确定辗扩比λ,根据给定的环件形状尺寸按经验选取辗扩比的范围,λ=du/d0,其中du和d0分别为环件凹槽部位的内径和毛坯的内径,λ的取值范围为2.0~2.5;
(2)根据凹槽环件尺寸、辗扩比和辗扩变形前后体积不变原理,确定矩形截面环形毛坯尺寸,凹槽环件体积为:
V = π H [ ( D - d 2 2 ) 2 - 1 3 ( H tan β ) 2 ] - 4 3 πR u 3 - 1 3 π ( H 2 - R u - h ) 3 sin 4 α 1 cos 2 α 1 - 8 3 πR u 3 tan 2 β - 1 3 π [ ( h 1 + 2 R u ) tan β - ( H 2 - R u - h ) ( sin 2 α 1 tan β - sinα 2 cosα 2 ) ] 2 [ h 1 - 2 R u - ( H 2 - R u - h ) sin 2 α 1 ] - 1 3 [ h 1 tan β - ( H 2 - R u - h ) sin 2 α 1 tan β ] 2 [ h 1 - ( H 2 - R u - h ) sin 2 α 1 ] - 2 πR u ( H 2 - R u - h ) 2 ( sinα 1 cosα 1 + sin 2 α 1 tan β ) 2
其中,D为环件外径,d2为斜内孔小内径,H为轴向高度,h为凹槽外沿与环件上下端面之间尺寸,h1为凹槽外沿高度,Ru为凹槽圆弧半径,α1、α2为凹槽上、下内壁与水平面夹角,β为斜内孔壁与环件轴向夹角;辗扩变形前后轴向高度尺寸不变,即毛坯高度H0=H,毛坯内径d0=du/λ,毛坯外径
(3)辗扩孔型设计:根据毛坯和环件的尺寸结构、截面形状及辗扩变形条件,设计驱动辊和芯辊的工作面型腔尺寸;驱动辊为主轧辊,其工作面型腔与凹槽环件截面形状对应,芯辊工作面设计为中部带外台阶形状,辗扩变形过程采用闭式孔型,芯辊外台阶沿环坯径向不断将其压入驱动辊工作面型腔;驱动辊与芯辊的工作面半径应满足:(1/RM1+1/RI)≤1.75θ/H0,RM1为驱动辊最大型腔位置半径,RI为芯辊外台阶半径,θ=tan-1μ为摩擦角,μ为摩擦系数,取值范围为0.5~0.7,RM1、RI根据总进给量Δh=[(D0-d0)-(D-du)]/2并结合与辗扩过程咬入条件和锻透条件的关系确定;芯辊外台阶高度与驱动辊工作面型腔高度一致,工作面型腔高度HM=H0+6~10mm,且为了提高辗扩时金属的流动性,设计型腔上、下内壁与水平面夹角γ为0°~6°;
(4)确定辗扩工艺参数,包括驱动辊转速、芯辊进给速度、初始辗扩温度以及辗扩终了温度,辗扩过程中驱动辊转速采用28.3~30.6r/min,芯辊进给速度采用不同的规范,咬入阶段进给速度由0mm/s增加到1.5mm/s,逐渐咬入形成凹槽轮廓,完成凹槽部位成形总量的30%;稳定辗扩阶段由1.5mm/s增加到2.0mm/s,快速辗扩得到凹槽完整形状,凹槽部位成形达到90%;精确校圆、整形阶段由2.0mm/s减小到0.5mm/s,对凹槽和斜内孔尺寸进行校整;根据锻造温度范围确定初始辗扩温度为1100~1150℃,并控制辗扩终了温度在870~900℃;
(5)辗扩成形:根据上述设计参数,在闭式辗环机上经过连续多道次变形使环坯直径不断扩大、斜内孔和凹槽截面辗扩成形。
CN201510611318.8A 2015-09-23 2015-09-23 一种凹槽斜内孔环件辗扩成形方法 Expired - Fee Related CN105127340B (zh)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN201510611318.8A CN105127340B (zh) 2015-09-23 2015-09-23 一种凹槽斜内孔环件辗扩成形方法

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN201510611318.8A CN105127340B (zh) 2015-09-23 2015-09-23 一种凹槽斜内孔环件辗扩成形方法

Publications (2)

Publication Number Publication Date
CN105127340A CN105127340A (zh) 2015-12-09
CN105127340B true CN105127340B (zh) 2017-03-22

Family

ID=54713098

Family Applications (1)

Application Number Title Priority Date Filing Date
CN201510611318.8A Expired - Fee Related CN105127340B (zh) 2015-09-23 2015-09-23 一种凹槽斜内孔环件辗扩成形方法

Country Status (1)

Country Link
CN (1) CN105127340B (zh)

Families Citing this family (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN106238632B (zh) * 2016-08-12 2018-01-05 西安航空职业技术学院 H形截面环件的辗扩成形方法
CN106984747B (zh) * 2016-12-01 2018-12-25 中国航发北京航空材料研究院 一种tc4合金内t形截面异形环件坯料的设计方法
CN106825339B (zh) * 2017-03-01 2018-10-26 西北工业大学 一种高温合金f型截面环件的异形坯料设计方法
CN110479923B (zh) * 2019-08-02 2020-08-25 武汉理工大学 大型薄壁外t形环状构件约束径轴向轧制成形方法
CN112989645B (zh) * 2021-01-24 2023-07-21 西北工业大学太仓长三角研究院 确定外表面有凹槽的异形环件轧制精确成形判据的方法

Family Cites Families (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN100396433C (zh) * 2005-07-22 2008-06-25 武汉理工大学 沟球截面环件冷辗扩成形方法
CN100337768C (zh) * 2005-10-24 2007-09-19 武汉理工大学 一次冷辗扩成形两个锥形截面环件的方法
KR101079729B1 (ko) * 2009-01-30 2011-11-04 손유홍 내경부의 이형 성형을 위한 링밀 장치 및 이를 이용한 이형링 제조방법
CN101829745B (zh) * 2010-04-23 2012-01-11 武汉理工大学 双沟槽截面环件冷辗扩成形的方法
JP5613468B2 (ja) * 2010-06-10 2014-10-22 Mmcスーパーアロイ株式会社 環状成形体の製造方法
CN102029341B (zh) * 2010-12-10 2012-10-03 贵州航宇科技发展股份有限公司 15CrMo钢薄壁环件的辗轧成形方法
CN102357531B (zh) * 2011-10-18 2013-10-02 武汉理工大学 一种厚壁深槽环件复合轧制成形工艺

Also Published As

Publication number Publication date
CN105127340A (zh) 2015-12-09

Similar Documents

Publication Publication Date Title
CN105127340B (zh) 一种凹槽斜内孔环件辗扩成形方法
CN102688962B (zh) 一种大型内台阶环件对称轧制成形方法
CN102489638B (zh) 一种大型内台阶环件径轴向轧制成形方法
CN102615221B (zh) 一种大型双沟槽环件径轴向轧制成形方法
CN102357531B (zh) 一种厚壁深槽环件复合轧制成形工艺
CN103316926A (zh) 一种l型截面汽车轮毂轴承环件冷轧成形方法
CN101687232B (zh) 通过冷轧法进行的超薄壁金属管的制造方法
CN104227349B (zh) 一种车轮轮辋制造方法
CN102836937A (zh) 厚壁小孔外台阶环件对称复合轧制成形方法
CN107545107A (zh) 一种用于梯形截面轴承环轧制的环坯及环坯设计方法
CN102500662A (zh) 大型管件整径矫圆方法
CN107931495A (zh) 一种筒形件的各向变形可控闭式轧制成形装置及方法
CN103230993B (zh) 一种确定圆锥台截面环件径向辗扩毛坯尺寸的方法
CN105363782A (zh) 张力减径机工作机组轧辊孔型
CN101829696A (zh) 一种中碳低合金结构钢的深孔挤压成形工艺
CN109590334B (zh) 主动锥齿轮轴毛坯楔横轧制模具及其轧制方法
CN104259354A (zh) 一种球阀法兰复合轧环成形方法
CN113680931A (zh) 大型内轮廓突变截面环件近净复合轧制成形方法
CN108568489A (zh) 一种圆锥滚子轴承外圈精密冷轧成形方法
CN102861840B (zh) 一种非对称双台阶回转体零件三辊横轧成形方法
CN201161255Y (zh) 适于生产高压锅炉用内螺纹钢管的模具
CN102172627A (zh) 一种复合绝缘子金具螺旋孔型斜轧轧辊孔型的设计方法
CN105382162B (zh) 空心钢锭预制的环状坯料的镦粗拔长方法
CN105215239B (zh) 一种凹槽斜内孔环件辗扩毛坯尺寸的设计方法
CN103302211A (zh) 小料头楔横轧工艺模具

Legal Events

Date Code Title Description
C06 Publication
PB01 Publication
C10 Entry into substantive examination
SE01 Entry into force of request for substantive examination
CB02 Change of applicant information

Inventor after: Qin Fangcheng

Inventor after: Li Yongtang

Inventor after: Liu Zhiqi

Inventor after: Qi Huiping

Inventor after: Li Zhi

Inventor before: Qin Fangcheng

Inventor before: Li Yongtang

Inventor before: Liu Zhiqi

Inventor before: Qi Huiping

CB03 Change of inventor or designer information
C14 Grant of patent or utility model
GR01 Patent grant
CF01 Termination of patent right due to non-payment of annual fee
CF01 Termination of patent right due to non-payment of annual fee

Granted publication date: 20170322

Termination date: 20170923