CN102771966B - Watch strap and manufacturing method thereof - Google Patents

Watch strap and manufacturing method thereof Download PDF

Info

Publication number
CN102771966B
CN102771966B CN201210222377.2A CN201210222377A CN102771966B CN 102771966 B CN102771966 B CN 102771966B CN 201210222377 A CN201210222377 A CN 201210222377A CN 102771966 B CN102771966 B CN 102771966B
Authority
CN
China
Prior art keywords
composite bed
base band
film
unit
unit composite
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201210222377.2A
Other languages
Chinese (zh)
Other versions
CN102771966A (en
Inventor
林韶孟
陈韶轩
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN201210222377.2A priority Critical patent/CN102771966B/en
Publication of CN102771966A publication Critical patent/CN102771966A/en
Application granted granted Critical
Publication of CN102771966B publication Critical patent/CN102771966B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种由硅胶制作的手表带及其制造方法,在该手表带至少一个表面印制的文字图案油墨层经久耐磨、不易脱落,其包括基带、由至少一个单元复合层构成的复合层,每个单元复合层由薄膜和印制在该薄膜内面上的文字图案油墨层构成,以文字图案油墨层叠置于所述基带表面与薄膜内表面之间的方式,经液态硫化或固态硫化成型法将复合层粘接或渗透在基带表面。本发明的手表带柔软且韧性好,其中,文字图案油墨层叠置在薄膜与硅胶基带之间,在高温作用下,所述文字图案油墨层、薄膜和基带三者之间结合紧密,本发明在薄膜上印刷文字图案时,采用规模化印刷,既降低了成本,又节省了时间。

The present invention discloses a watch band made of silicone and a manufacturing method thereof. The text pattern ink layer printed on at least one surface of the watch band is durable and wear-resistant and not easy to fall off. The watch band includes a base band and a composite layer composed of at least one unit composite layer. Each unit composite layer is composed of a film and a text pattern ink layer printed on the inner surface of the film. The text pattern ink layer is stacked between the surface of the base band and the inner surface of the film, and the composite layer is bonded or infiltrated on the surface of the base band by liquid vulcanization or solid vulcanization molding. The watch band of the present invention is soft and has good toughness. The text pattern ink layer is stacked between the film and the silicone base band. Under the action of high temperature, the text pattern ink layer, the film and the base band are tightly combined. When printing the text pattern on the film, the present invention adopts large-scale printing, which not only reduces costs but also saves time.

Description

手表带及其制造方法Watch strap and manufacturing method thereof

技术领域technical field

本发明涉及手表配件,特别涉及一种表面印有经久耐磨文字图案的硅胶表带及制造该表带的方法。The invention relates to watch accessories, in particular to a silicone watch strap with a durable and wear-resistant character pattern printed on the surface and a method for manufacturing the watch strap.

背景技术Background technique

现有技术中,手表带上的文字图案油墨层都是用丝印或水转印方法将文字图案油墨层印制在手表带的外表面上,然后再在所述的文字图案油墨层上喷涂一层薄薄的涂层(以下称保护层),以此来保护印在手表带上的文字图案油墨层不脱落,但是由于所述保护层、油墨层和手表带三者之间结合不紧密,在佩带手表的过程中,由于表带会与袖口或衣服经常摩擦,手表带外表面上的保护层很容易破损,由此,导致印制在手表带外表面上的文字图案油墨层脱落,从而使手表带显得陈旧,大大影响手表带产品的使用价值和市场占有率,另外,现有技术中手表带上文字图案的印刷是在已制作好的手表带上一条一条的印制,待文字图案的油墨干燥后再逐条涂敷保护层,此方法不仅费时、费力、费财,而且干燥后的文字图案油墨与手表带表面的结合力较小很易脱落。In the prior art, the text and pattern ink layer on the watch strap is printed on the outer surface of the watch strap by silk screen printing or water transfer printing, and then sprays a layer of ink on the text and pattern ink layer. A thin layer of coating (hereinafter referred to as protective layer) protects the ink layer printed on the watch strap from coming off, but because the protective layer, the ink layer and the watch strap are not tightly combined, In the process of wearing a watch, because the watch strap will often rub against the cuffs or clothes, the protective layer on the outer surface of the watch strap is easily damaged, thus causing the ink layer of the text and pattern printed on the outer surface of the watch strap to fall off, thereby It makes the watch strap look obsolete, which greatly affects the use value and market share of the watch strap product. In addition, the printing of the text and pattern on the watch strap in the prior art is to print one by one on the watch strap that has been made. After the ink is dry, apply the protective layer one by one. This method is not only time-consuming, laborious, and expensive, but also the dried text and pattern ink has a small bonding force with the surface of the watch strap and is easy to fall off.

发明内容Contents of the invention

本发明要解决的技术问题是提供一种由硅胶材料制作的手表带,在该手表带的至少一个表面上印制的文字图案油墨层经久耐磨、不易脱落以及制造该手表带的方法。The technical problem to be solved by the present invention is to provide a watch strap made of silica gel material, the ink layer of the printed characters and patterns on at least one surface of the watch strap is durable and not easy to fall off, and a method for manufacturing the watch strap.

本发明采用的技术方案为:The technical scheme adopted in the present invention is:

本发明的手表带,包括基带、由文字图案和外层保护层构成的贴敷在基带表面的膜层,所述基带为硅胶所制,所述膜层为由至少一个单元复合层构成的复合层,每个单元复合层均由薄膜制作的所述的外层保护层和印制在该薄膜内面上的由文字图案油墨层制作的所述的文字图案构成,所述复合层以文字图案油墨层叠置于所述薄膜内面与基带表面之间的方式,采用热压工艺经液态硫化成型法或固态硫化成型法粘接或渗透在基带的表面上;The watch band of the present invention comprises a base band, a film layer composed of a character pattern and an outer protective layer and attached to the surface of the base band. Layer, each unit composite layer is made of the described outer protective layer made of film and the described text pattern printed on the inner surface of the film made of text pattern ink layer, the composite layer is made of text pattern ink The layers are placed between the inner surface of the film and the surface of the base tape, and are bonded or penetrated on the surface of the base tape through a liquid vulcanization molding method or a solid vulcanization molding method using a hot pressing process;

所述文字图案油墨层是由文字图案层和粘合剂层组合而成,所述的粘合剂层是热溶胶膜或涂层;The text pattern ink layer is composed of a text pattern layer and an adhesive layer, and the adhesive layer is a hot melt film or coating;

所述的热溶胶膜或涂层为TPU热溶胶膜或涂层、EVA热溶胶膜或涂层、OPP热溶胶膜或涂层、PA热溶胶膜或涂层。The hot-melt film or coating is TPU hot-melt film or coating, EVA hot-melt film or coating, OPP hot-melt film or coating, PA hot-melt film or coating.

在所述基带的内外两个表面上均设有所述复合层。The composite layer is provided on both inner and outer surfaces of the base belt.

所述复合层有二个单元复合层。The composite layer has two unit composite layers.

所述的薄膜为树脂或硅胶所制。The film is made of resin or silica gel.

制造本发明所述手表带的方法,先将文字图案油墨印制在已制备好的薄膜的内表面上形成带有文字图案油墨层的单元复合层;再将该单元复合层或者由多个该单元复合层按上一个单元复合层的文字图案油墨层与下一个单元复合层的薄膜相接顺序依次叠置构成的复合层,以文字图案油墨层叠置于所述基带表面与薄膜内表面之间的方式,采用热压工艺将所述单元复合层或者复合层与基带表面紧密结合在一起;The method for manufacturing the wristband of the present invention is as follows: firstly print the text and pattern ink on the inner surface of the prepared film to form a unit composite layer with the text and pattern ink layer; then the unit composite layer or a plurality of such The unit composite layer is a composite layer formed by sequentially stacking the text and pattern ink layer of the previous unit composite layer and the film of the next unit composite layer, and the text and pattern ink layer is stacked between the surface of the base tape and the inner surface of the film In a way, the unit composite layer or the composite layer and the surface of the base tape are closely combined by a hot pressing process;

所述文字图案油墨层是由文字图案层和粘合剂层组合而成,所述的粘合剂层是热溶胶膜或涂层;The text pattern ink layer is composed of a text pattern layer and an adhesive layer, and the adhesive layer is a hot melt film or coating;

所述的热溶胶膜或涂层为TPU热溶胶膜或涂层、EVA热溶胶膜或涂层、OPP热溶胶膜或涂层、PA热溶胶膜或涂层。The hot-melt film or coating is TPU hot-melt film or coating, EVA hot-melt film or coating, OPP hot-melt film or coating, PA hot-melt film or coating.

本发明的将所述基带与单元复合层或者复合层相结合的第一种方法有以下步骤:The first method of combining the base tape with the unit composite layer or the composite layer of the present invention has the following steps:

第一步,将单元复合层或者复合层置于表带模具的模腔内,单元复合层或者复合层中的薄膜紧贴模腔底壁,文字图案油墨层朝向模腔内预留的空间;In the first step, the unit composite layer or the composite layer is placed in the mold cavity of the strap mould, the unit composite layer or the film in the composite layer is close to the bottom wall of the mold cavity, and the text pattern ink layer faces the reserved space in the mold cavity;

第二步,将双组分硅胶溶胶液体注入所述模具的模腔内;In the second step, the two-component silica gel sol liquid is injected into the mold cavity of the mold;

第三步,将所述模具温度升至90-180℃,硫化时间在0.4-2分钟,使液态硅胶转化为固态基带并与单元复合层或者复合层粘合;In the third step, the temperature of the mold is raised to 90-180°C, and the vulcanization time is 0.4-2 minutes, so that the liquid silica gel is converted into a solid base tape and bonded to the unit composite layer or the composite layer;

第四步,打开所述模具将已制好的由基带和单元复合层或者复合层构成的手表带取出即可。The fourth step is to open the mold and take out the finished wristband composed of the base band and the unit composite layer or the composite layer.

本发明第一种方法中所述模具温度优选为140℃。The mold temperature in the first method of the present invention is preferably 140°C.

本发明的将所述基带与单元复合层或者复合层相结合的第二种方法有以下步骤:The second method of combining the baseband with the unit composite layer or the composite layer of the present invention has the following steps:

第一步,将单元复合层或者复合层置于表带模具的模腔内,单元复合层或者复合层中的薄膜紧贴模腔底壁,文字图案油墨层朝向模腔内预留的空间;In the first step, the unit composite layer or the composite layer is placed in the mold cavity of the strap mould, the unit composite layer or the film in the composite layer is close to the bottom wall of the mold cavity, and the text pattern ink layer faces the reserved space in the mold cavity;

第二步,将已混合好的固态硅胶放置于所述模腔内,合上模具;In the second step, the mixed solid silica gel is placed in the mold cavity, and the mold is closed;

第三步,将所述模具温度升至120~200℃,保持0.8-3分钟的时间,使硅胶硫化成基带并与复合层5粘合;In the third step, the temperature of the mold is raised to 120-200° C., and kept for 0.8-3 minutes, so that the silica gel is vulcanized into a base tape and bonded to the composite layer 5;

第四步,打开所述模具将已制好的由基带和单元复合层或者复合层构成的手表带取出即可。The fourth step is to open the mold and take out the finished wristband composed of the base band and the unit composite layer or the composite layer.

第二种方法中所述的模具温度优选为170℃。The mold temperature described in the second method is preferably 170°C.

本发明的将所述基带与单元复合层或者复合层相结合的第三种方法有以下步骤:The third method of combining the baseband with the unit composite layer or the composite layer of the present invention has the following steps:

第一步,将单元复合层或者复合层置于表带模具的模腔内,单元复合层或者复合层中的薄膜紧贴模腔底壁,文字图案油墨层朝向模腔内预留的空间;In the first step, the unit composite layer or the composite layer is placed in the mold cavity of the strap mould, the unit composite layer or the film in the composite layer is close to the bottom wall of the mold cavity, and the text pattern ink layer faces the reserved space in the mold cavity;

第二步,将已制好的基带的一面紧贴所述的单元复合层或者复合层放入所述模腔内;In the second step, one side of the prepared base tape is placed in the mold cavity close to the unit composite layer or the composite layer;

第三步,再将另一片制好的单元复合层或者复合层紧贴所述基带的另一面放入所述模腔内,合上模具;The third step is to put another unit composite layer or the composite layer close to the other side of the base tape into the mold cavity, and close the mold;

第四步,将所述模具温度升至90-200℃,保持1-30秒的时间,使单元复合层或者复合层与基带粘合;The fourth step is to raise the temperature of the mold to 90-200°C and keep it for 1-30 seconds to bond the unit composite layer or the composite layer to the base tape;

第五步,打开所述模具将已制好的由基带和单元复合层或者复合层构成的手表带取出即可。The fifth step is to open the mold and take out the finished wristband composed of the base band and the unit composite layer or the composite layer.

与现有技术相比,本发明采用液态硫化成型法或者固态硫化成型法,将由文字图案油墨层和一定厚度的薄膜构成的复合层与硅胶材料制作的基带紧密的结合在一起,所制的手表带柔软且韧性好,其中,文字图案油墨层叠置在薄膜与硅胶基带之间,在高温作用下,所述文字图案油墨层、薄膜和基带三者之间结合紧密,使得印制在本发明手表带上的文字图案经久耐用、不易脱落,而且,所述文字图案在所述薄膜的保护下能够长时间保持原有的光泽和色彩,当本发明的复合层为多个单元复合层构成时,其上的文字图案层更加经久耐用,使用寿命更长。本发明在薄膜上印刷文字图案时,采用规模化印刷,既降低了成本,又节省了时间。Compared with the prior art, the present invention uses a liquid vulcanization molding method or a solid vulcanization molding method to closely combine a composite layer composed of a text pattern ink layer and a film of a certain thickness with a base band made of silica gel material, and the watch manufactured The tape is soft and has good toughness, wherein, the text pattern ink layer is stacked between the film and the silica gel base band, and under the action of high temperature, the text pattern ink layer, the film and the base band are closely combined, so that the printed on the watch of the present invention The characters and patterns on the belt are durable and not easy to fall off, and the characters and patterns can keep the original luster and color for a long time under the protection of the film. When the composite layer of the present invention is composed of multiple unit composite layers, The text pattern layer on it is more durable and has a longer service life. The present invention adopts large-scale printing when printing characters and patterns on the film, which not only reduces the cost, but also saves time.

附图说明Description of drawings

下面结合附图和具体实施方式对本发明作进一步的详细说明。The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

图1为本发明的示意图。Figure 1 is a schematic diagram of the present invention.

图2为图1中A-A剖视放大图。Fig. 2 is an enlarged cross-sectional view of A-A in Fig. 1 .

图3为图2中的文字图案油墨层局剖放大图。FIG. 3 is an enlarged partial cross-sectional view of the text and pattern ink layer in FIG. 2 .

具体实施方式Detailed ways

如图1、2所示,本发明的手表带,是由手表基带1、印有文字图案的复合层5构成。As shown in Figures 1 and 2, the watch band of the present invention is composed of a watch base band 1 and a composite layer 5 printed with text and patterns.

所述基带1是由硅胶材料所制,所述硅胶为液体硅胶、液体硅橡胶、乙烯基硅橡胶、低苯基硅橡胶或氟硅硅橡胶。The base belt 1 is made of silica gel material, and the silica gel is liquid silica gel, liquid silicone rubber, vinyl silicone rubber, low phenyl silicone rubber or fluorosilicone silicone rubber.

所述复合层5由至少一个单元复合层4构成,每个单元复合层4是由文字图案油墨层3和具有一定厚度的薄膜2构成。The composite layer 5 is composed of at least one unit composite layer 4, and each unit composite layer 4 is composed of a character pattern ink layer 3 and a film 2 with a certain thickness.

所述文字图案油墨层3是由文字图案层6和/或粘合剂层7组合而成。The character pattern ink layer 3 is composed of a character pattern layer 6 and/or an adhesive layer 7 .

所述的文字图案层6,是由油墨印刷或涂布而制成。The character pattern layer 6 is made by ink printing or coating.

所述的粘合剂层7可以是热溶胶膜或涂层、热硫化胶粘剂涂层或热硫化催化剂涂层。其作用是在液态或固态硫化时,将树脂薄膜或硅胶薄膜、文字图案层6和硅胶基带1粘合在一起。The adhesive layer 7 can be a hot melt film or coating, a thermal vulcanization adhesive coating or a thermal vulcanization catalyst coating. Its function is to bond the resin film or silica gel film, text pattern layer 6 and silica gel base tape 1 together during liquid or solid vulcanization.

所述文字图案层6的内容是根据客户需求而定,通常,是手表带生产商的名称、手表带的型号、规格、商标或者艺术图案等代表商业信息或显示表带外观艺术美的至少一种。The content of the text pattern layer 6 is determined according to customer needs, usually, it is at least one of the name of the watch strap manufacturer, the model, specification, trademark or artistic pattern, etc. that represent business information or show the artistic beauty of the watch strap appearance. .

所述粘合剂层7既用于将文字图案层6与薄膜2相互粘接或渗透(经热压方法)构成单元复合层4,也用于将多个单元复合层4粘接或渗透(经热压方法)构成复合层5,还用于将所述单元复合层4或者复合层5与基带1表面紧密粘接或渗透(经热硫化或热压方法)在一起。Said adhesive layer 7 is both used for bonding or infiltrating the text pattern layer 6 and the film 2 mutually (through hot pressing method) to form the unit composite layer 4, and is also used for bonding or infiltrating a plurality of unit composite layers 4 ( hot pressing method) to form the composite layer 5, which is also used to closely bond or infiltrate the unit composite layer 4 or the composite layer 5 and the surface of the base tape 1 (by hot vulcanization or hot pressing method).

所述粘合剂层7所用的热溶胶膜或涂层、热硫化胶粘剂涂层或热硫化催化剂涂层分别为:The hot melt film or coating, heat vulcanization adhesive coating or heat vulcanization catalyst coating used in the adhesive layer 7 are respectively:

所用的热溶胶膜或涂层为TPU热溶胶膜或涂层、EVA热溶胶膜或涂层、OPP热溶胶膜或涂层、PA热溶胶膜或涂层;The hot melt film or coating used is TPU hot melt film or coating, EVA hot melt film or coating, OPP hot melt film or coating, PA hot melt film or coating;

所用的热硫化胶粘剂层是由热溶胶体或树脂胶体与铂金催化剂混合而成;The thermal vulcanization adhesive layer used is formed by mixing hot melt colloid or resin colloid with platinum catalyst;

所用的热硫化催化剂层也是由热溶胶体或树脂胶体与铂金催化剂混合而成;The thermal vulcanization catalyst layer used is also made of hot melt colloid or resin colloid mixed with platinum catalyst;

所述薄膜2是由树脂或硅胶材料所制的透明薄膜,其具有一定的厚度,厚度在0.03-1.0微米,所用树脂为TPU(英文全称:Thermoplastic polyurethanes,中文名称:热塑性聚氨酯弹性体塑胶)、PET(中文名;聚对苯二甲酸乙二醇酯为高聚合物,英文名:polyethyleneterephthalate)、PVC(中文名:聚氯乙烯英文名:Polyvinylchloride,)、PE(英文全称:Polyethylene,中文名:聚乙烯)等。The film 2 is a transparent film made of resin or silica gel material, which has a certain thickness of 0.03-1.0 microns, and the resin used is TPU (English full name: Thermoplastic polyurethanes, Chinese name: thermoplastic polyurethane elastomer plastic), PET (Chinese name; polyethylene terephthalate is a high polymer, English name: polyethyleneterephthalate), PVC (Chinese name: polyvinyl chloride English name: Polyvinylchloride), PE (English name: Polyethylene, Chinese name: polyethylene), etc.

每个单元复合层4是由如下方法制作:采用丝印、胶印或数码打印方法将文字图案油墨印制在已制备好的整张薄膜上,然后覆上粘合剂层7,再将其切割制成表带形状的单元复合层4。Each unit composite layer 4 is made by the following method: use silk screen printing, offset printing or digital printing to print the text and pattern ink on the prepared whole film, then cover the adhesive layer 7, and then cut it A unit composite layer 4 in the shape of a watch strap.

所述复合层5是将多个所述单元复合层4按上一个单元复合层4的文字图案油墨层3与相邻的下一个单元复合层4的薄膜2相接的顺序依次叠置经热压而成。Described composite layer 5 is that a plurality of described unit composite layers 4 are stacked sequentially through heat in the order that the character pattern ink layer 3 of the last unit composite layer 4 is connected to the film 2 of the adjacent next unit composite layer 4. Pressed.

本发明中的复合层5可以是一个单元复合层4,也可以是多个单元复合层4,优选为二个单元复合层4。The composite layer 5 in the present invention can be one unit composite layer 4 or multiple unit composite layers 4 , preferably two unit composite layers 4 .

所述复合层5是以文字图案油墨层3叠置于所述薄膜2内面与基带1表面之间的方式,经液态硫化成型法或固态硫化成型法粘接或渗透在基带1的表面上。The composite layer 5 is bonded or infiltrated on the surface of the base tape 1 through liquid vulcanization molding or solid vulcanization molding in such a way that the text and pattern ink layer 3 is stacked between the inner surface of the film 2 and the surface of the base tape 1 .

本发明手表带的复合层5设置在所述基带1的内表面和/或外表面上。The composite layer 5 of the wristband of the invention is arranged on the inner and/or outer surface of said base band 1 .

由于采用液态硫化成型法或固态硫化成型法制作本发明,经高温硫化,所述复合层5牢牢粘接甚至部分渗透在硅胶基带1的表层内,将文字图案油墨层3、薄膜2与基带1紧密的结合在一起,确保文字图案油墨层3在硅胶基带1表面的持久性,所制的手表带柔软且韧性好,手表带上的文字图案经久耐用、不易脱落。Since the present invention is produced by liquid vulcanization molding method or solid vulcanization molding method, after high temperature vulcanization, the composite layer 5 is firmly bonded and even partly penetrates into the surface layer of the silica gel base tape 1, and the text pattern ink layer 3, the film 2 and the base tape 1 are closely combined to ensure the persistence of the text and pattern ink layer 3 on the surface of the silicone base band 1, and the watch band is soft and tough, and the text and pattern on the watch band are durable and not easy to fall off.

本发明手表带的制作方法之一,由以下步骤构成:One of the manufacturing methods of the watch strap of the present invention consists of the following steps:

第一步,采用丝印、胶印或数码打印方法将文字图案油墨印制在已制备好的整张薄膜上,然后覆上所述的粘合剂层7,再将其切割制成表带形状的单元复合层4;In the first step, use silk screen printing, offset printing or digital printing to print the text and pattern ink on the prepared whole film, then cover the above-mentioned adhesive layer 7, and then cut it into a strap-shaped unit composite layer 4;

第二步,将该单元复合层4置于表带模具的模腔内,单元复合层4的薄膜2紧贴模腔底壁,文字图案油墨层3朝向模腔内预留的空间;In the second step, the unit composite layer 4 is placed in the mold cavity of the strap mould, the film 2 of the unit composite layer 4 is close to the bottom wall of the mold cavity, and the text pattern ink layer 3 faces the reserved space in the mold cavity;

或者将由多个所述单元复合层4按上一个单元复合层4的文字图案油墨层3与相邻的下一个单元复合层4的薄膜2相接顺序依次叠置经热压构成的复合层5,置于表带模具的模腔内,复合层5中最外层的薄膜2紧贴模腔底壁,最里层的文字图案油墨层3朝向模腔内预留的空间;Or by a plurality of said unit composite layers 4, press the character pattern ink layer 3 of the last unit composite layer 4 and the film 2 of the adjacent next unit composite layer 4 to be stacked successively through the composite layer 5 formed by hot pressing , placed in the mold cavity of the strap mold, the outermost film 2 in the composite layer 5 is close to the bottom wall of the mold cavity, and the innermost text pattern ink layer 3 faces the reserved space in the mold cavity;

第三步,将双组分的硅胶(俗称AB硅胶)溶胶液体注入所述模具的模腔内;In the third step, a two-component silica gel (commonly known as AB silica gel) sol liquid is injected into the mold cavity of the mould;

第三步,将所述模具温度升至90-180℃,优选温度为140℃,硫化时间在0.4-2分钟,使液态硅胶硫化转化为固态基带并通过所述的粘合剂层7与复合层5紧密粘合在一起;In the third step, the temperature of the mold is raised to 90-180°C, preferably 140°C, and the vulcanization time is 0.4-2 minutes, so that the liquid silica gel can be vulcanized and converted into a solid base tape and compounded with the adhesive layer 7 Layer 5 is tightly bonded together;

第四步,打开所述模具将已制好的由基带1和单元复合层4或者复合层5构成的手表带取出即可。The fourth step is to open the mold and take out the finished wristband composed of the base band 1 and the unit composite layer 4 or composite layer 5 .

本发明手表带的制作方法之二,由以下步骤构成:The second manufacturing method of the watch strap of the present invention consists of the following steps:

第一步,采用丝印、胶印或数码打印方法将文字图案油墨印制在已制备好的整张薄膜上,然后覆上粘合剂层7,再将其切割制成表带形状的单元复合层4;The first step is to print the text and pattern ink on the prepared whole film by silk screen printing, offset printing or digital printing, then cover the adhesive layer 7, and then cut it into a watchband-shaped unit composite layer 4;

第二步,将该单元复合层4置于表带模具的模腔内,单元复合层4的薄膜2紧贴模腔底壁,文字图案油墨层3朝向模腔内预留的空间;In the second step, the unit composite layer 4 is placed in the mold cavity of the strap mould, the film 2 of the unit composite layer 4 is close to the bottom wall of the mold cavity, and the text pattern ink layer 3 faces the reserved space in the mold cavity;

或者将由多个所述单元复合层4按上一个单元复合层4的文字图案油墨层3与相邻的下一个单元复合层4的薄膜2相接顺序依次叠置经热压构成的复合层5,置于表带模具的模腔内,复合层5中最外层的薄膜2紧贴模腔底壁,最里层的文字图案油墨层3朝向模腔内预留的空间;Or by a plurality of said unit composite layers 4, press the character pattern ink layer 3 of the last unit composite layer 4 and the film 2 of the adjacent next unit composite layer 4 to be stacked successively through the composite layer 5 formed by hot pressing , placed in the mold cavity of the strap mold, the outermost film 2 in the composite layer 5 is close to the bottom wall of the mold cavity, and the innermost text pattern ink layer 3 faces the reserved space in the mold cavity;

第三步,将已混合好的固态硅胶放置于所述的模腔内,合上模具;The third step is to place the mixed solid silica gel in the mold cavity and close the mold;

第四步,将所述模具温度升至120~200℃,优选温度为170℃,保持0.8-3分钟的时间,使硅胶硫化成基带并通过所述的粘合剂层7与复合层5紧密粘合在一起;The fourth step is to raise the temperature of the mold to 120-200°C, preferably 170°C, and keep it for 0.8-3 minutes, so that the silica gel can be vulcanized into a base tape and tightly bonded to the composite layer 5 through the adhesive layer 7 stick together;

第四步,打开所述模具将已制好的由基带1和单元复合层4或者复合层5构成的手表带取出即可。The fourth step is to open the mold and take out the finished wristband composed of the base band 1 and the unit composite layer 4 or composite layer 5 .

本发明手表带的制作方法之三,由以下步骤构成:The third manufacturing method of watch band of the present invention consists of the following steps:

第一步,采用丝印、胶印或数码打印方法将文字图案油墨印制在已制备好的整张薄膜上,然后覆上粘合剂层7,再将其切割制成表带形状的单元复合层4;The first step is to print the text and pattern ink on the prepared whole film by silk screen printing, offset printing or digital printing, then cover the adhesive layer 7, and then cut it into a watchband-shaped unit composite layer 4;

第二步,将该单元复合层4置于表带模具的模腔内,单元复合层4的薄膜2紧贴模腔底壁,文字图案油墨层3朝向模腔内预留的空间;In the second step, the unit composite layer 4 is placed in the mold cavity of the strap mould, the film 2 of the unit composite layer 4 is close to the bottom wall of the mold cavity, and the text pattern ink layer 3 faces the reserved space in the mold cavity;

或者将由多个所述单元复合层4按上一个单元复合层4的文字图案油墨层3与相邻的下一个单元复合层4的薄膜2相接顺序依次叠置经热压构成的复合层5,置于表带模具的模腔内,复合层5中最外层的薄膜2紧贴模腔底壁,最里层的文字图案油墨层3朝向模腔内预留的空间;Or by a plurality of said unit composite layers 4, press the character pattern ink layer 3 of the last unit composite layer 4 and the film 2 of the adjacent next unit composite layer 4 to be stacked successively through the composite layer 5 formed by hot pressing , placed in the mold cavity of the strap mold, the outermost film 2 in the composite layer 5 is close to the bottom wall of the mold cavity, and the innermost text pattern ink layer 3 faces the reserved space in the mold cavity;

第三步,将已制好的硅胶基带的一面紧贴所述的单元复合层4或者复合层5放入所述模腔内;In the third step, one side of the prepared silica gel base tape is placed in the mold cavity close to the unit composite layer 4 or the composite layer 5;

第四步,再将另一片制好的单元复合层4或者复合层5紧贴所述基带的另一面放入所述模腔内,合上模具;The fourth step is to put another prepared unit composite layer 4 or composite layer 5 into the mold cavity close to the other side of the base tape, and close the mold;

第四步,将所述模具温度升至90-200℃,优选温度为180℃,保持1-30秒的时间,使所述硅胶基带通过粘合剂层7与设于其两面上的复合层5紧密粘结在一起;The fourth step is to raise the temperature of the mold to 90-200°C, preferably 180°C, and keep it for 1-30 seconds, so that the silicone base tape passes through the adhesive layer 7 and the composite layers on both sides. 5 tightly bonded together;

第五步,打开所述模具将已制好的由基带1和单元复合层4或者复合层5构成的手表带取出即可。The fifth step is to open the mold and take out the finished wristband composed of the base band 1 and the unit composite layer 4 or composite layer 5 .

Claims (10)

1. a watchband, comprise base band (1), the rete sticking on base band surface be made up of character pattern and outer protective layer, it is characterized in that: described base band (1) for silica gel made, described rete is the composite bed (5) be made up of at least one unit composite bed (4), the described outer protective layer that each unit composite bed (4) makes by film (2) and be printed on the described character pattern that this film (2) inner face is made by character pattern ink layer (3) and form, described composite bed (5) is stacked and placed on the mode between described film (2) inner face and base band (1) surface with character pattern ink layer (3), employing heat pressing process is through liquid sulfidization molding method or solid-state sulfidization molding method is bonding or permeate on the surface of base band (1),
Described character pattern ink layer (3) is combined by word graph pattern layer (6) and adhesive phase (7), and described adhesive phase (7) is thermosol glued membrane or coating;
Described thermosol glued membrane or coating are TPU thermosol glued membrane or coating, EVA thermosol glued membrane or coating, OPP thermosol glued membrane or coating, PA thermosol glued membrane or coating.
2. watchband according to claim 1, is characterized in that: on inside and outside two surfaces of described base band (1), be equipped with described composite bed (5).
3. watchband according to claim 1, is characterized in that: described composite bed (5) has two unit composite beds (4).
4. the watchband according to any one of claim 1-3, is characterized in that: described film (2) for resin or silica gel made.
5. a method for the watchband described in manufacturing claims 1, is characterized in that: the inner surface first character pattern ink being printed on the film (2) prepared is formed the unit composite bed (4) with character pattern ink layer (3); To connect with the film (2) of next unit composite bed (4) the order stacked composite bed (5) formed successively by this unit composite bed (4) or by this unit composite bed (4) multiple by the character pattern ink layer (3) of a upper unit composite bed (4) again, be stacked and placed on the mode between described base band (1) surface and film (2) inner surface with character pattern ink layer (3), adopt heat pressing process described unit composite bed (4) or composite bed (5) to be combined with base band (1) intimate surface;
Described character pattern ink layer (3) is combined by word graph pattern layer (6) and adhesive phase (7), and described adhesive phase (7) is thermosol glued membrane or coating;
Described thermosol glued membrane or coating are TPU thermosol glued membrane or coating, EVA thermosol glued membrane or coating, OPP thermosol glued membrane or coating, PA thermosol glued membrane or coating.
6. method according to claim 5, is characterized in that: described base band (1) and unit composite bed (4) or composite bed (5) be combined with following steps:
The first step, unit composite bed (4) or composite bed (5) are placed in the die cavity of watchband mould, film (2) in unit composite bed (4) or composite bed (5) is close to die cavity diapire, the space that character pattern ink layer (3) is reserved in die cavity;
Second step, injects in the die cavity of described mould by double-component silicon sol liquid;
3rd step, rises to 90-180 DEG C by described mold temperature, and cure time, at 0.4-2 minute, makes liquid-state silicon gel be converted into solid-state base band (1) and bonds with unit composite bed (4) or composite bed (5);
4th step, opens described mould and is taken out by the watchband be made up of base band (1) and unit composite bed (4) or composite bed (5) made.
7. method according to claim 6, is characterized in that: described temperature is 140 DEG C.
8. method according to claim 5, is characterized in that: described base band (1) and unit composite bed (4) or composite bed (5) be combined with following steps:
The first step, unit composite bed (4) or composite bed (5) are placed in the die cavity of watchband mould, film (2) in unit composite bed (4) or composite bed (5) is close to die cavity diapire, the space that character pattern ink layer (3) is reserved in die cavity;
Second step, is positioned in described die cavity by the solid-state silica gel mixed, closed die;
3rd step, rises to 120 ~ 200 DEG C by described mold temperature, keeps the time of 0.8-3 minute, makes silica gel be sulfided into base band and bond with composite bed 5;
4th step, opens described mould and is taken out by the watchband be made up of base band (1) and unit composite bed (4) or composite bed (5) made.
9. method according to claim 8, is characterized in that: described temperature is 170 DEG C.
10. method according to claim 5, is characterized in that: described base band (1) and unit composite bed (4) or composite bed (5) be combined with following steps:
The first step, unit composite bed (4) or composite bed (5) are placed in the die cavity of watchband mould, film (2) in unit composite bed (4) or composite bed (5) is close to die cavity diapire, the space that character pattern ink layer (3) is reserved in die cavity;
Second step, is close to described unit composite bed (4) by the one side of the base band made or composite bed (5) puts into described die cavity;
3rd step, then the another side that the unit composite bed (4) made by another sheet or composite bed (5) are close to described base band puts into described die cavity, closed die;
4th step, rises to 90-200 DEG C by described mold temperature, keeps the time of 1-30 second, and unit composite bed (4) or composite bed (5) are bonded with base band;
5th step, opens described mould and is taken out by the watchband be made up of base band (1) and unit composite bed (4) or composite bed (5) made.
CN201210222377.2A 2012-06-29 2012-06-29 Watch strap and manufacturing method thereof Expired - Fee Related CN102771966B (en)