CN102688901B - 一种08Mn钢板板形控制的方法 - Google Patents
一种08Mn钢板板形控制的方法 Download PDFInfo
- Publication number
- CN102688901B CN102688901B CN201210195350.9A CN201210195350A CN102688901B CN 102688901 B CN102688901 B CN 102688901B CN 201210195350 A CN201210195350 A CN 201210195350A CN 102688901 B CN102688901 B CN 102688901B
- Authority
- CN
- China
- Prior art keywords
- steel plate
- thickness
- billet
- straightening
- control
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
本发明提供一种08Mn钢板板形控制的方法,根据钢坯厚度确定在炉时间及均热温度:采用单机架轧制成品厚度在40mm以上钢板时,最后两个成型道次的轧制力控制在3500-4500t;采用3道矫直工艺,并根据钢板厚度不同采用不同的输入厚度、弯辊形式和弯辊力。从而可保证08Mn钢坯加热温度的均匀一致性,提高钢坯表面的除鳞效果,避免钢板尾部的“碎浪”缺陷,改善矫直过程中钢板内应力释放及相变的条件,有效提高矫直效果,使08Mn成品钢板的板形合格率由88.75%提高到98.99%,回矫率大幅度降低,显著降低生产成本。
Description
技术领域
本发明属于轧钢工艺技术领域,尤其涉及一种用于轧制08Mn中厚钢板时板型控制的方法。
背景技术
低合金08Mn中厚钢板由于其具有在保证高强度的情况下,仍保持较高的韧性和焊接性能,因此近年来已广泛应用于石油管、舰船、大型结构件及海洋设施等领域,并受到高度重视。然而,在生产过程中发现,对于采用单机架轧制的中厚板厂来说,原有的控制手段已难以满足08Mn中厚钢板的生产需要,致使08Mn中厚钢板的板形合格率仅为88.75%,每月产生的板形问题造成的回矫率高达1.25%以上,不仅直接影响产品质量合格率,而且严重影响生产流程和生产成本。
究其板形合格率低的主要原因,一是加热制度不尽合理。由于08Mn轧制钢板要求低温加热,开轧温度偏低,因而无法保证钢坯温度的均匀性和除鳞效果所致。二是目前采用的是半自动轧制,压下量由二级计算机给定,在轧制08Mn钢板时,由于荷重较大,二级计算机计算后道次较多、压下量较小,导致较厚的钢板尾部极易产生“碎浪”缺陷,直接影响表面质量合格率。
发明内容
本发明的目的旨在提供一种可改善08Mn钢板板形,提高板形合格率,减少轧制废品的08Mn钢板板形控制的方法。
为此,本发明所采取的解决方案是:
一种08Mn钢板板形控制的方法,其具体控制方法为:
1、加热制度控制:
根据钢坯厚度确定在炉时间及均热温度:
230mm厚钢坯,在炉时间为4-4.5h,均热温度为1160-1170℃;
300mm厚钢坯,在炉时间为4.5-5h,均热温度为1230-1240℃;
2、轧制力控制:
采用单机架轧制钢板厚度在40mm以上钢板时,最后两个成型道次的轧制力控制在3500-4500t;
3、矫直参数控制:
采用3道矫直工艺;
根据钢板厚度不同采用的具体矫直参数为:
钢板厚度(mm) | 输入厚度(mm) | 弯辊方式 | 弯辊力(kN) |
12-15 | 比实际厚度减0.5 | 正弯 | +1.6~+1.8 |
16-32 | 按实际厚度 | 按正常模型给定 | 按正常模型给定 |
>32 | 比实际厚度加0.5 | 负弯 | -1.0~-1.5 |
本发明的有益效果为:
由于本发明采取了上述综合性措施,从而可保证08Mn钢坯加热温度的均匀一致性,提高钢坯表面的除鳞效果;合理控制轧制压力,调整压下量,避免钢板尾部的“碎浪”缺陷;优化矫直参数和弯辊形式,改善了矫直过程中钢板内应力释放及相变的条件,有效提高了矫直效果,使08Mn成品钢板的板形合格率由88.75%提高到98.99%,回矫率大幅度降低,轧制废品明显减少,显著降低了生产成本。
具体实施方式
实施例1:
08Mn钢坯厚度230mm,生产钢板厚度为14mm,其具体控制方法为:
1、加热制度控制:
在炉时间为4h,均热温度为1160℃。
2、矫直参数控制:
采用3道矫直工艺;
根据钢板厚度不同采用的具体矫直参数为:
钢板厚度(mm) | 输入厚度(mm) | 弯辊方式 | 弯辊力(kN) |
14 | 13.5 | 正弯 | +1.75 |
实施例2:
08Mn钢坯厚度230mm,生产钢板厚度为25mm,其具体控制方法为:
1、加热制度控制:
在炉时间为4.4h,均热温度为1170℃。
2、矫直参数控制:
采用3道矫直工艺;
根据钢板厚度不同采用的具体矫直参数为:
钢板厚度(mm) | 输入厚度(mm) | 弯辊方式 | 弯辊力(kN) |
25 | 25 | 按正常模型给定 | 按正常模型给定 |
实施例3:
08Mn钢坯厚度300mm,生产钢板厚度为55mm,其具体控制方法为:
1、加热制度控制:
在炉时间为4.8h,均热温度为1230℃。
2、轧制力控制:
采用单机架轧制,最后两个成型道次的轧制力控制在4100t。
3、矫直参数控制:
采用3道矫直工艺;
根据钢板厚度不同采用的具体矫直参数为:
钢板厚度(mm) | 输入厚度(mm) | 弯辊方式 | 弯辊力(kN) |
55 | 55.5 | 负弯 | -1.3 |
Claims (1)