CN102533372A - Briquettes produced by using recovered material discharged from industrial boilers as raw material and production method thereof - Google Patents
Briquettes produced by using recovered material discharged from industrial boilers as raw material and production method thereof Download PDFInfo
- Publication number
- CN102533372A CN102533372A CN2012100058501A CN201210005850A CN102533372A CN 102533372 A CN102533372 A CN 102533372A CN 2012100058501 A CN2012100058501 A CN 2012100058501A CN 201210005850 A CN201210005850 A CN 201210005850A CN 102533372 A CN102533372 A CN 102533372A
- Authority
- CN
- China
- Prior art keywords
- coal
- water
- kindling
- discharge
- reclaims
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses briquettes, which are produced by using a recovered material discharged from industrial boilers as a raw material and by adding clay, desulfurizer, waterproofing agent and auxiliary materials (coal slime, blind coal, coke powder, mixed coal, fly ash, straw, bran, furnace slag and the like). According to raw material mixing ratio, the briquettes fall into three classes: 1, long-flame coal (4,000 to 6,000 kilocalories) which is prepared from 80 to 90 percent of main material, 2 to 5 percent of clay, 3 to 5 percent of desulfurizer, 2 to 4 percent of waterproofing agent, 3 to 5 percent of auxiliary material and 1 to 3 percent of water; 2, medium-flame coal (3,000 to 4,000 kilocalories) which is prepared from 60 to 80 percent of main material, 5 to 10 percent of clay, 3 to 5 percent of desulfurizer, 3 to 5 percent of waterproofing agent, 10 to 25 percent of auxiliary material and 1 to 3 percent of water; and 3, thermal-insulation coal (2,000 to 3,000 kilocalories) which is prepared from 40 to 60 percent of main material, 5 to 13 percent of clay, 3 to 5 percent of desulfurizer, 3 to 5 percent of waterproofing agent, 20 to 45 percent of auxiliary material and 1 to 3 percent of water.
Description
Technical field
The present invention relates to a kind of solid fuel and working method thereof, belong to the fuel manufacture field, refer to that specifically a kind of discharge that reclaims with Industrial Boiler makes the Type Coal And Its Production Methods of main raw material production.
Background technology
At present, the technology of producing moulded coal is a lot, wherein mainly with hard coal, mixed coal, coke powder, flyash, biological raw material (straw, sawdust etc.), furfural, coal gangue, coal slime etc. as main raw material.Add subsidiary material such as sulphur-fixing agent, water-resisting agent, solidifying agent in addition again and produce, these methods, consumes energy are too high, but heat is not high, and are on fire too slow during burning; Also have present Mainstream Packs product of coal all to use coal slime, coal slime is settled out in the raw coal cleaning process, contains a large amount of impurity (being ash); The quality of raw coal is low more, and the heat of coal slime is low more, and the impurity that coal slime contains is bigger (ash is big more) just; The quality product of producing is just unstable; Heat is also unstable, and the pollution of discharging is just big, and the harm of environment is still existed.
Summary of the invention
The present invention is directed to above-mentioned having now all is the problem that technology exists, and has proposed a kind of discharge that reclaims with Industrial Boiler and has made the moulded coal of main raw material production, and proposed the working method of above-mentioned moulded coal.
A kind of discharge that reclaims with Industrial Boiler of the present invention is made the moulded coal of main raw material production, it is characterized in that through regulating the proportioning of main raw material, the moulded coal that can produce three kinds of labels promptly 1, go up kindling 4000-6000 kilocalorie; 2, middle kindling 3000-4000 kilocalorie; 3, insulation coal 2000-3000 kilocalorie.
A kind of discharge that reclaims with Industrial Boiler of the present invention is made the moulded coal of main raw material production, it is characterized in that mainly comprising the component of following three kinds of label moulded coals:
One, upward the principal character of kindling comprises following material mixture ratio (weight ratio: part)
The discharge 80-90% that Industrial Boiler reclaims; Clay 2-5%; Sweetening agent 3-5%; Water-resisting agent 2-4%; Other subsidiary material 3-5% (coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc.), water 1-3%.
Two, the principal character of middle kindling comprises following material mixture ratio (weight ratio: part)
The discharge 60-80% that Industrial Boiler reclaims; Clay 5-10%; Sweetening agent 3-5%; Water-resisting agent 3-5%; Other subsidiary material 10-25% (coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc.), water 1-3%.
Three, the principal character of insulation coal comprises following material mixture ratio (weight ratio: part)
The discharge 40-60% that Industrial Boiler reclaims; Clay 5-13%; Sweetening agent 3-5%; Water-resisting agent 3-5%; Other subsidiary material 20%-45% (coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc.), water 1-3%.
Described a kind of discharge that reclaims with Industrial Boiler is made the moulded coal of raw material production, it is characterized in that described sweetening agent is a lime powder, its content 1, last kindling 3-5%; 2, middle kindling 3-5%; 3, insulation coal 3-5%.Said water-resisting agent is a flyash, its content 1, last kindling 2-4%; 2, middle kindling 3-5%; 3, insulation coal 3-5%.The content of the discharge that described Industrial Boiler reclaims is 1, go up kindling 80-90%; Middle kindling 60-80%; Insulation coal 40-60%.Described clay is a soil property of firing clay brick, and its content is 1, goes up kindling 2-5%; 2, middle kindling 5-10%; 3, insulation coal 5-13%.Described subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment equal size are 1, go up kindling 3-5%; 2, middle kindling 10-25%; 3, insulation coal 20-45%.Described water is 1-3%.
Realize that the above-mentioned discharge that reclaims with Industrial Boiler makes the method for the moulded coal of raw material production, it is characterized in that:
1, the discharge dry (methods such as Exposure to Sunlight, natural ventilation, oven dry) that Industrial Boiler is reclaimed, water ratio about 16%;
2, with clay somely be crushed to below 50 orders, sweetening agent (lime powder) is crushed to below 50 orders, subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc. are crushed to below 50; The discharge of getting the Industrial Boiler recovery is some, carries out the moulded coal preparation of following three kinds of labels.
A, last kindling: (4000-6000 kilocalorie)
A, get the discharge that the Industrial Boiler of 80-90% weight part reclaims;
B, interpolation clay 2-5% weight part, sweetening agent 3-5% weight part, water-resisting agent 2-4% weight part;
C, add 3-5% weight parts such as other subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment again, water 1-3% weight part (can extrusion molding to be as the criterion) stirs, and forms the moulded coal mixing raw material
D, with the extrusion molding in the die forming machine of making a gift to someone of above-mentioned moulded coal mixing raw material, squeeze pressure 2-3MP;
E, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio are less than 10%.
B, middle kindling: (3000-4000 kilocalorie)
A, get the discharge that the Industrial Boiler of 60-80% weight part reclaims;
B, interpolation clay 5-10% weight part, sweetening agent 3-5% weight part, water-resisting agent 3-5% weight part;
C, add 10-25% weight parts such as other subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment again, water 1-3% weight part (can extrusion molding to be as the criterion) stirs, and forms the moulded coal mixing raw material
D, with the extrusion molding in the die forming machine of making a gift to someone of above-mentioned moulded coal mixing raw material, squeeze pressure 2-3MP;
E, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio are less than 10%.
C, insulation coal: (2000-3000 kilocalorie)
A, get the discharge that the Industrial Boiler of 40-60% weight part reclaims;
B, interpolation clay 5-13% weight part, sweetening agent 3-5% weight part, water-resisting agent 3-5% weight part;
C, add 20-45% weight parts such as other subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment again, water 1-3% weight part (can extrusion molding to be as the criterion) stirs, and forms the moulded coal mixing raw material
D, with the extrusion molding in the die forming machine of making a gift to someone of above-mentioned moulded coal mixing raw material, squeeze pressure 2-3MP;
E, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio are less than 10%.
3, dried moulded coal just becomes finished product, is carried out to pile buttress warehouse-in.
The discharge that reclaims with Industrial Boiler of the present invention is made the moulded coal of main raw material production, in raw material, has added sweetening agent, water-resisting agent has increased water-repellancy, has reduced the discharging of sulphur, has reduced environmental pollution.The subsidiary material that in raw material, add conveniently are prone to get, and when producing, can also gather materials on the spot, and turn waste into wealth, and reduce raw materials cost.Utilize the cohesiveness of self simultaneously, increased the intensity of moulded coal, reduced the breakage of loading and unloading, transportation.When extruding, adopted at present popular Totally-enclosed-type briquette shaping machine the most, pressure is big, has improved the degree of compactness and the intensity of moulded coal, and production efficiency is also along with having improved.
Embodiment
Below the discharge that reclaims with Industrial Boiler of the present invention is made raw material production moulded coal be described in detail.
Moulded coal of the present invention is a main raw material with the discharge that Industrial Boiler reclaims; Add the part clay as sticker, this clay is that general clay that can brickmaking get final product, and the water-resisting agent of interpolation is the cheap flyash of using always at present; Effect is to prevent moulded coal chance water distortion or defeated and dispersed; The lime powder that adds is as sweetening agent, can reduce the discharging of sulfurous gas, plays the effect of solid sulphur; Under clean-burning condition, reduce more than 95% when the discharging of sulfurous gas is burnt separately than other subsidiary material.Because the discharge self that Industrial Boiler reclaims has fixed effect, moulded coal burning back shape invariance, the convenient removing.
The moulded coal method that the discharge that reclaims with Industrial Boiler of the present invention is a main material production is fairly simple, with the discharge dry (methods such as Exposure to Sunlight, natural ventilation, oven dry) that Industrial Boiler reclaims, water ratio about 16%; With clay powder be broken to below 50 orders, sweetening agent (lime powder) is crushed to below 50 orders, subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc. are crushed to below 50 orders; Extrusion equipment has adopted at present popular Totally-enclosed-type briquette shaping machine the most.Carry out the moulded coal of following three kinds of labels makes through embodiment
One, goes up kindling (4000-6000 kilocalorie)
Embodiment 1
Get 80 tons of discharge main raw materials that Industrial Boiler reclaims, add 5 tons of clays (below 50 orders), 5 tons of lime powders (below 50 orders), 5 tons in flyash, add 2 tons of 5 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 2
Get 83 tons of discharge main raw materials that Industrial Boiler reclaims, add 3.5 tons of clays (below 50 orders), 3.5 tons of lime powders (below 50 orders), 5 tons in flyash, add 2 tons of 5 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 3
Get 88 tons of discharge main raw materials that Industrial Boiler reclaims, add 4 tons of clays (below 50 orders), 3 tons of lime powders (below 50 orders), 4 tons in flyash, add 2 tons of 1 ton of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 4
Get 90 tons of discharge main raw materials that Industrial Boiler reclaims, add 3 tons of clays (below 50 orders), 3 tons of lime powders (below 50 orders), 3 tons in flyash, add 2 tons of 1 ton of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Two, middle kindling (3000-4000 kilocalorie)
Embodiment 1
Get 60 tons of discharge main raw materials that Industrial Boiler reclaims, add 10 tons of clays (below 50 orders), 5 tons of lime powders (below 50 orders), 5 tons in flyash, add 2 tons of 20 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 2
Get 65 tons of discharge main raw materials that Industrial Boiler reclaims, add 6 tons of clays (below 50 orders), 4 tons of lime powders (below 50 orders), 4 tons in flyash, add 2 tons of 21 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 3
Get 70 tons of discharge main raw materials that Industrial Boiler reclaims, add 4 tons of clays (below 50 orders), 3 tons of lime powders (below 50 orders), 3 tons in flyash, add 2 tons of 20 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 4
Get 75 tons of discharge main raw materials that Industrial Boiler reclaims, add 5 tons of clays (below 50 orders), 3 tons of lime powders (below 50 orders), 3 tons in flyash, add 2 tons of 14 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Three, insulation coal (2000-3000 kilocalorie)
Embodiment 1
Get 40 tons of discharge main raw materials that Industrial Boiler reclaims, add 13 tons of clays (below 50 orders), 5 tons of lime powders (below 50 orders), 5 tons in flyash, add 2 tons of 37 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 2
Get 45 tons of discharge main raw materials that Industrial Boiler reclaims, add 10 tons of clays (below 50 orders), 5 tons of lime powders (below 50 orders), 5 tons in flyash, add 2 tons of 35 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 3
Get 50 tons of discharge main raw materials that Industrial Boiler reclaims, add 10 tons of clays (below 50 orders), 5 tons of lime powders (below 50 orders), 5 tons in flyash, add 2 tons of 30 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Embodiment 4
Get 55 tons of discharge main raw materials that Industrial Boiler reclaims, add 8 tons of clays (below 50 orders), 5 tons of lime powders (below 50 orders), 5 tons in flyash, add 2 tons of 27 tons of subsidiary material coal slimes (or hard coal or coke powder or mixed coal or flyash or straw or furfural or boiler ash sediment), water (can extrusion molding to be as the criterion) again; Stir; Moulded coal mixing raw material after stirring is sent into extrusion molding in the whole-enclosed coal die forming machine; Squeeze pressure 2-3MP; Produce 100 tons of moulded coals, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio can dispatch from the factory less than 10% o'clock.
Claims (5)
1. a discharge that reclaims with Industrial Boiler is made the moulded coal of main raw material production, it is characterized in that through regulating the proportioning of main raw material, the moulded coal that can produce three kinds of labels promptly 1, go up kindling 4000-6000 kilocalorie; 2, middle kindling 3000-4000 kilocalorie; 3, insulation coal 2000-3000 kilocalorie.
2. make the moulded coal of main raw material production according to a kind of discharge that reclaims with Industrial Boiler of claim 1, it is characterized in that mainly comprising the proportioning raw materials of following three kinds of label moulded coals:
One, upward the principal character of kindling comprises following proportioning raw materials (weight ratio: part)
The discharge 80-90% that Industrial Boiler reclaims; Clay 2-5%; Sweetening agent 3-5%; Water-resisting agent 2-4%; Other subsidiary material 3-5% (coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc.), water 1-3%;
Two, the principal character of middle kindling comprises following proportioning raw materials (weight ratio: part)
The discharge 60-80% that Industrial Boiler reclaims; Clay 5-10%; Sweetening agent 3-5%; Water-resisting agent 3-5%; Other subsidiary material 10-25% (coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc.), water 1-3%;
Three, the principal character of insulation coal comprises following proportioning raw materials (weight ratio: part)
The discharge 40-60% that Industrial Boiler reclaims; Clay 5-13%; Sweetening agent 3-5%; Water-resisting agent 3-5%; Other subsidiary material 20%-45% (coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc.), water 1-3%.
3.
,The discharge that reclaims with Industrial Boiler according to claim 2 is the moulded coal of main material production, it is characterized in that described sweetening agent is a lime powder, its content 1, last kindling 3-5%; 2, middle kindling 3-5%; 3, insulation coal 3-5%; Said water-resisting agent is a flyash, its content 1, last kindling 2-4%; 2, middle kindling 3-5%; 3, insulation coal 3-5%; The content of the discharge that described Industrial Boiler reclaims is 1, go up kindling 80-90%; Middle kindling 60-80%; Insulation coal 40-60%; Described clay is a soil property of firing clay brick, and its content is 1, goes up kindling 2-5%; 2, middle kindling 5-10%; 3, insulation coal 5-13%; Described subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment equal size are 1, go up kindling 3-5%; 2, middle kindling 10-25%; 3, insulation coal 20-45%; Described water is 1-3%.
4.
,The discharge that reclaims with Industrial Boiler according to claim 3 is the moulded coal of main material production, it is characterized in that the discharge self that described Industrial Boiler reclaims has cohesive action.
5.
,A kind ofly realize among the claim 1-4 that each said discharge that reclaims with Industrial Boiler is the working method of the moulded coal of main material production, it is characterized in that:
1), discharge dry (methods such as Exposure to Sunlight, natural ventilation, oven dry) that Industrial Boiler is reclaimed, water ratio about 16%;
2), with clay somely be crushed to below 50 orders, sweetening agent (lime powder) is crushed to below 50 orders, subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment etc. are crushed to below 50; The discharge of getting the Industrial Boiler recovery is some, carries out the moulded coal preparation of following three kinds of labels;
A, last kindling: (4000-6000 kilocalorie)
A, get the discharge that the Industrial Boiler of 80-90% weight part reclaims;
B, interpolation clay 2-5% weight part, sweetening agent 3-5% weight part, water-resisting agent 2-4% weight part;
C, add 3-5% weight parts such as other subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment again, water 1-3% weight part (can extrusion molding to be as the criterion) stirs, and forms the moulded coal mixing raw material
D, with the extrusion molding in the die forming machine of making a gift to someone of above-mentioned moulded coal mixing raw material, squeeze pressure 2-3MP;
E, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio are less than 10%;
B, middle kindling: (3000-4000 kilocalorie)
A, get the discharge that the Industrial Boiler of 60-80% weight part reclaims;
B, interpolation clay 5-10% weight part, sweetening agent 3-5% weight part, water-resisting agent 3-5% weight part;
C, add 10-25% weight parts such as other subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment again, water 1-3% weight part (can extrusion molding to be as the criterion) stirs, and forms the moulded coal mixing raw material
D, with the extrusion molding in the die forming machine of making a gift to someone of above-mentioned moulded coal mixing raw material, squeeze pressure 2-3MP;
E, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio are less than 10%;
C, insulation coal: (2000-3000 kilocalorie)
A, get the discharge that the Industrial Boiler of 40-60% weight part reclaims;
B, interpolation clay 5-13% weight part, sweetening agent 3-5% weight part, water-resisting agent 3-5% weight part;
C, add 20-45% weight parts such as other subsidiary material coal slime, hard coal, coke powder, mixed coal, flyash, straw, furfural, boiler ash sediment again, water 1-3% weight part (can extrusion molding to be as the criterion) stirs, and forms the moulded coal mixing raw material
D, with the extrusion molding in the die forming machine of making a gift to someone of above-mentioned moulded coal mixing raw material, squeeze pressure 2-3MP;
E, demoulding after drying (Exposure to Sunlight, natural ventilation, oven dry etc.) water ratio are less than 10%.