[go: up one dir, main page]

CN101701123A - Preparation method of vitrified colorful stone lacquer - Google Patents

Preparation method of vitrified colorful stone lacquer Download PDF

Info

Publication number
CN101701123A
CN101701123A CN200910073165A CN200910073165A CN101701123A CN 101701123 A CN101701123 A CN 101701123A CN 200910073165 A CN200910073165 A CN 200910073165A CN 200910073165 A CN200910073165 A CN 200910073165A CN 101701123 A CN101701123 A CN 101701123A
Authority
CN
China
Prior art keywords
preparation
stone lacquer
vitrified
mixed solution
colored stone
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN200910073165A
Other languages
Chinese (zh)
Inventor
王家财
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN200910073165A priority Critical patent/CN101701123A/en
Publication of CN101701123A publication Critical patent/CN101701123A/en
Pending legal-status Critical Current

Abstract

The invention discloses a preparation method of vitrified colorful stone lacquer, relating to coating. The method solves the problems that: existing stone lacquer has serious dust absorption and fading obscission, particularly contains more carbonate stone which can perform chemical reaction in air and then is dissolved when meeting water, thereby causing color change, crude true stone lacquer spraying surface, easy dust adhesion and uneasy dust elimination. The method of the invention comprises the following steps: firstly, mixing vitrified micro beads with inorganic ceramic pigment, and sintering into colorful micro beads under high temperature condition; secondly, mixing and stirring penetration agent and antiager by weight percent and then preparing into opacifying mixed liquor, mixing the mixed liquor and thickener emulsion until mutual solubility, and then evenly stirring with styrene-acrylate emulsion; and thirdly, evenly mixing 50-80% of vitrified beads and 20-50% of mixed liquid by weight percent to obtain vitrified stone paint. The invention has the advantages of true stone lacquer such as naturalness, primitive simplicity, dazzling beauty, fresh and elegance, cleanness and environment protection, light weight and wear resistance, various colors and permanent color.

Description

A kind of preparation method of glass colored stone lacquer
Technical field
The present invention relates to the preparation of coating.Relate in particular to the preparation method of glass color coating material.
Background technology
Existing material of construction is to develop and develop along with real estate and living standards of the people improve, exterior coating is of a great variety, people pursue the theory of environment-friendly natural, expedite the emergence of out a lot of novel decorative coating, the true mineral varnish that the nineties is risen, because the thick and heavy nature of its texture is subjected to pursuing of people, and the trend of replacement marble-ceramic tile is arranged greatly, because of it is that the natural crystal pulverizing processes, look that effect is fine, but after using 1~2 year, dust is serious and have the obscission of fading to take place, natural rock is impure many, especially contain stone material, chemical reaction, CaCO can take place in air by more carbonate 3+ H 2O+CO 2=Ca (HCO 3) 2, Ca (HCO 3) 2Meeting water can dissolve, and this is the major cause that causes color to change, and true in addition mineral varnish sprayed surface is coarse, and is not ageing-resistant, and not environmental protection adheres to the dust and the problem of easy-clear not easily.
Summary of the invention
The present invention is that the natural crystal pulverizing processes in order to solve existing mineral varnish because of it, look that effect is fine, but after using 1~2 year, dust is serious and have the obscission of fading to take place, natural rock is impure many, especially contain stone material, chemical reaction, CaCO can take place in air by more carbonate 3+ H 2O+CO 2=Ca (HCO 3) 2, Ca (HCO 3) 2Meeting water can dissolve, this is the major cause that causes color to change, true in addition mineral varnish sprayed surface is coarse, not ageing-resistant, not environmental protection, adhere to the dust and the problem of easy-clear not easily, and a kind of preparation method of glass colored stone lacquer is provided, and the concrete technical scheme that addresses this problem is as follows:
The preparation method's of a kind of glass colored stone lacquer of the present invention step is as follows:
Step 1, glass bead and inorganic ceramic pigment are mixed by weight 6.5~7.5: 1~2.5, put into electrical heater and under 550~850 ℃ of conditions, be fired into vitrified color balls;
Step 2, by weight percentage permeate agent (permeate agent employing peregal) be 0.2~1% and antiaging agent be 0.1~0.5% mix to stir and to make the milkiness mixed solution, mixed solution again with by weight percentage high-quality thickening material (Mierocrystalline cellulose) be 8~11% emulsions mix dissolve each other after, be that acrylic tackifier stirs and gets final product with surplus again;
Step 3, vitrified color balls and mixed solution that step 1 and step 2 are obtained, vitrified color balls is 50~80% by weight percentage, mixed solution is 20~50% to stir after mixing and promptly make glass colored stone lacquer of the present invention.
The color exterior coating of glass of the present invention, the color microballon of glass adds permeate agent, tinting material adopts inorganic ceramic pigment, oxidation and corrosion, the high-temperature firing clinkering together, can not with airborne any substance reaction; The effect of permeate agent is to promote the infiltration of tackiness agent and coating for wall surface to merge, and has effectively improved cohesive strength, and antiaging agent can prevent tackiness agent by the corrosion of acid, alkali, oxygen obnoxious flavour, and can reach 30 years the work-ing life that acrylic acid or the like strengthens tackiness agent; It also has natural, simple and unsophisticated, dazzlingly beautiful, the pure and fresh elegance, solid thick and heavy of true mineral varnish, and clean environment firendly, light weight are wear-resisting, significantly reduced the load-bearing on heat-preserving wall surface, also have simultaneously firm durable, glittering and translucent, color is various, the durable advantage more than 30 years of color.The present invention compares with marble with ceramic tile; easy construction is quick; time saving and energy saving, coating is firmly hard after solidifying, and can clean at any time; stupalith is fully tasteless nontoxic; after the high temperature vitreous, sealing of hole cover in addition is so surface-brightening is level and smooth; do not soak, do not glue ash, clean light, improved the quality and the class of material of construction.Now authentication detects in the national chemical building material of process test center.
Embodiment
Embodiment one: the preparation method's of the glass colored stone lacquer of present embodiment step is as follows:
Step 1, glass bead and inorganic ceramic pigment are mixed by weight 6.5~7.5: 1~2.5, put into electrical heater and under 550~850 ℃ of conditions, be fired into vitrified color balls;
Step 2, by weight percentage permeate agent (permeate agent employing peregal) be 0.2~1% and antiaging agent be 0.1~0.5% mix to stir and to make the milkiness mixed solution, mixed solution again with by weight percentage high-quality thickening material (Mierocrystalline cellulose) be 8~11% emulsions mix dissolve each other after, be that stir gets final product acrylic tackifier (acrylic tackifier adopt pure third or benzene emulsion) with surplus again;
Step 3, vitrified color balls and mixed solution that step 1 and step 2 are obtained, vitrified color balls is 50~80% by weight percentage, mixed solution is 20~50% to stir after mixing and promptly make glass colored stone lacquer of the present invention.
Embodiment two: present embodiment is glass bead in the step 1 is mixed by weight 7: 2 with inorganic ceramic pigment with the difference of embodiment one, puts into electrical heater and be fired into vitrified color balls under 700 ℃ of conditions.
Embodiment three: present embodiment and the difference of embodiment one be in the step 2 by weight percentage permeate agent be 0.5% and protective agent be 0.3% to mix to stir and make the milkiness mixed solution, mixed solution again with the high-quality Mierocrystalline cellulose be 10% emulsion mix dissolve each other after, be that pure-acrylic emulsion stirs and gets final product with surplus again.
Embodiment four: present embodiment and the difference of embodiment one are in the step 3 by weight percentage that vitrified color balls is 65%, mixed solution is 35% to stir after mixing and promptly make glass colored stone lacquer of the present invention.

Claims (7)

1. the preparation method of glass colored stone lacquer is characterized in that this preparation method's step is as follows:
Step 1, glass bead and inorganic ceramic pigment are mixed by weight 6.5~7.5: 1~2.5, put into electrical heater and under 550~850 ℃ of conditions, be fired into vitrified color balls;
Step 2, by weight percentage permeate agent be 0.2~1% and antiaging agent be 0.1~0.5% mix to stir and to make the milkiness mixed solution, mixed solution again with by weight percentage high-quality thickening material be 8~11% emulsions mix dissolve each other after, be that acrylic tackifier stirs and gets final product with surplus again;
Step 3, vitrified color balls and mixed solution that step 1 and step 2 are obtained, vitrified color balls is 50~80% by weight percentage, mixed solution is 20~50% to stir after mixing and promptly make glass colored stone lacquer of the present invention.
2. the preparation method of a kind of glass colored stone lacquer according to claim 1 is characterized in that permeate agent adopts peregal.
3. the preparation method of a kind of glass colored stone lacquer according to claim 1 is characterized in that thickening material selects Mierocrystalline cellulose for use.
4. the preparation method of a kind of glass colored stone lacquer according to claim 1 is characterized in that acrylic tackifier adopts pure third or benzene emulsion.
5. the preparation method of a kind of glass colored stone lacquer according to claim 1 is characterized in that glass bead in the step 1 is mixed by weight 7: 2 with inorganic ceramic pigment, puts into electrical heater and be fired into vitrified color balls under 700 ℃ of conditions.
6. the preparation method of a kind of glass colored stone lacquer according to claim 1, it is characterized in that in the step 2 by weight percentage permeate agent be 0.5% and protective agent be 0.3% to mix to stir and make the milkiness mixed solution, mixed solution again with Mierocrystalline cellulose be 10% emulsion mix dissolve each other after, be that pure-acrylic emulsion stirs and gets final product with surplus again.
7. the preparation method of a kind of glass colored stone lacquer according to claim 1 is characterized in that in the step 3 by weight percentage that vitrified color balls is 65%, mixed solution is 35% to stir after mixing and promptly make glass colored stone lacquer of the present invention.
CN200910073165A 2009-11-10 2009-11-10 Preparation method of vitrified colorful stone lacquer Pending CN101701123A (en)