[go: up one dir, main page]

CN101255325A - Synthesis technique of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive - Google Patents

Synthesis technique of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive Download PDF

Info

Publication number
CN101255325A
CN101255325A CNA2007100377332A CN200710037733A CN101255325A CN 101255325 A CN101255325 A CN 101255325A CN A2007100377332 A CNA2007100377332 A CN A2007100377332A CN 200710037733 A CN200710037733 A CN 200710037733A CN 101255325 A CN101255325 A CN 101255325A
Authority
CN
China
Prior art keywords
component
parts
weight
dual
add
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CNA2007100377332A
Other languages
Chinese (zh)
Inventor
李岿然
周平
张蕙兰
李新军
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SHANGHAI HUAXIA CHEMICAL MATERIALS CO Ltd
Original Assignee
SHANGHAI HUAXIA CHEMICAL MATERIALS CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SHANGHAI HUAXIA CHEMICAL MATERIALS CO Ltd filed Critical SHANGHAI HUAXIA CHEMICAL MATERIALS CO Ltd
Priority to CNA2007100377332A priority Critical patent/CN101255325A/en
Publication of CN101255325A publication Critical patent/CN101255325A/en
Pending legal-status Critical Current

Abstract

The invention provides a double-component, heat and humidity resistance epoxy architecture reinforcement glue, comprising first and second components. The preparation method of the glue comprises: 1) adding reactive toughening agent thiocol, fluid epoxy resin, reactive diluent C12-14 tertiary carbonic acid ethylene oxidic ester, reactive diluent phenyl glycidyl ether and antifoaming agent by weight portion, silane coupler, discharged gas phase white carbon black and uniformly stirring, standing and defoaming to obtain first compnent: 2) uniformly stirring the isophorone diamine, metaxylene diamine, aromatic alcohol, salicylic acid and epoxy resin E44 to obtain second component curing agent by weight portion; mixing the promoter and curing agent in proportion to obtain second component. The architecture reinforcement glue without solvent can be cured at room temperature and conveniently constructed, with fine viscosity, good thixotropy, excellent resistance to heat and humidity, mechanical property and adhesive property, without toxin and pollution.

Description

A kind of synthesis technique of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive
Technical field
The present invention relates to the structural strengthening glue that a kind of building trade is used, relate in particular to the epoxy construction reinforced glue of wet and heat ageing resistant.
Background technology
National standard " concrete structure reinforcement design specifications " is middle regulation (GB50367-2006): the Steel Concrete load larrying member are reinforced and are sticked with glue agent, steel-steel bonding shear behavior must be up to the standards through hydrothermal aging, and the requirement that meets aspects such as environmental protection construction colloidal property, but existing building structural strengthening glue has the following disadvantages on use and performance own:
Makeup of the imports reinforced glue curing cross-linking reaction is slow, and the construction time is long; Low temperature does not solidify, and meets weather in the construction process and turns cold and will additionally take to be incubated the heating measure; Initial bond strenght is lower, influences adhesive effect and on-site construction operations, and costs an arm and a leg, and the building reinforce cost is big, and the user is difficult to bear.
Homemade structural strengthening glue wet and heat ageing resistant poor performance, fragility is big, and poor toughness, mechanical property do not reach the construction structure glue A grade standard of national up-to-date promulgation, can't satisfy the key state project construction requirement; In use can not adjust working life, very short time in summer inner structure glue gelatin phenomenon just takes place, be unfavorable for that big area reinforces; When temperature is lower than 10 ℃ the construction time long, gel not even below 0 ℃, influence construction.
And have the solvent of contaminate environment and harmful solidifying agent in the structural strengthening glue moiety mostly, be unfavorable for environmental protection and workmen's health.
Summary of the invention
Problem to be solved by this invention provides a kind of safety and environmental protection, moderate cost, excellent performance, meet national standard, can be applicable to the wet and heat ageing resistant building structure strengthening adhesive of the structural strengthening of all kinds of state keys buildings and covil construction.
For addressing the above problem, the present invention is achieved in that a kind of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive, is made of the first and second two kinds of components, and synthesis technique is:
(1) preparation of first component
A. add 0.5~2 part of endurable active toughener thiorubber, liquid-state epoxy resin E51 or 12875~120 parts in the agitator by weight, stirring at normal temperature is even;
B. add reactive thinner C more by weight 12-1468000.1~1 parts of 6~8 parts of tertiary carbonic acid glycidyl esters (hereinafter to be referred as E-10), 6~8 parts of reactive thinner phenyl glycidyl ethers (hereinafter to be referred as PGE) and defoamer Defom, stirring at normal temperature is even;
C. add 0.5~2 part of silane coupling agent (KH560) by weight in the described liquid of step (1) b, stirring at normal temperature is even;
D. add 1~2 part of the white carbon black of hydrophobic gas phase by weight in the described liquid of step (1) c, stir, with 1400~2000 rev/mins of high-speed stirring 15 minutes, leave standstill froth breaking and promptly get the first component again until no visible meal;
(2) preparation of second component
A. in the reaction vessel by weight with 70~95 parts of isophorone diamines (hereinafter to be referred as IPDA), 5~30 parts of m-xylene diamines (hereinafter to be referred as MXDA), left standstill after mixing 10 minutes;
B. add 60~90 parts of aromatic alcohols, 5~15 parts of catalyzer Whitfield's ointments more by weight successively, stir mixed in 30 minutes after, be added dropwise to step (2) a gained liquid, dropwise in one and a half hours;
C. add Resins, epoxy E4410~30 part in step (2) the b gained liquid by weight, keep temperature to mix half an hour below 40 ℃, second component solidifying agent;
D. by weight altax P-301~3 part are joined in 40~80 parts of described second component solidifying agent, stirred 10 minutes, promptly get the second component.
First component and the matching used weight proportion of second component are 1.5: 1 to 3: 1.
Described aromatic alcohol is a phenylcarbinol, or is phenylethyl alcohol.
Usually stirring velocity is 700 rev/mins, and churning time is 3~5 minutes.
Advantage of the present invention is: two-pack wet and heat ageing resistant building structure strengthening adhesive of the present invention self-vulcanizing, modest viscosity, easy construction, thixotropic property is good, have advantages such as excellent wet and heat ageing resistant performance, mechanical property, bond properties, nontoxic pollution-free, its characteristics are:
1. has excellent wet and heat ageing resistant performance.Adopt IPDA, MXDA to make this structure glue have more phenyl ring, alicyclic structure, the resistance toheat height; IPDA makes to contain in the second component and contains the white carbon black of hydrophobic gas phase in more methyl group and the first component, and hydrophobicity is good; Ring texture such as phenyl ring and alicyclic ring makes the cured article compact structure, and waterproof gas-tight performance is good.
2. applied widely, this structure glue has Applicable temperature scope and dried wet scope widely, and low-temperature curable all can be used in-10 ℃~40 ℃ scopes, and the rainy day construction is unaffected.
3. shrinking percentage is low, and this glue shrinking percentage is 0.3~0.5%, is 1/2~1/5 of other like product, and shear-stress is little, not easy to crack between composite fibre layer behind feasible curing the and building member, and consolidation effect is good.
4. dielectric behavior excellences such as acid and alkali-resistance and anti-oil, kerosene, salt solution, long service life.
5. the present invention is solvent-free construction structure glue, nontoxic pollution-free in construction and the use.
Embodiment
The present invention is described in more detail according to specific embodiment below: the material endurable active toughener thiorubber JLY-121 that adopts among the embodiment is Daopu Chemical International Trade Co., Ltd., Shanghai's product, and reactive thinner E-10 is the sharp worker company limited product that foreignizes in Shanghai; Reactive thinner PGE and altax P-30 are Shenzhen Jia Dida chemical industry company limited product; Silane coupling agent KH560 fastens the general chemical of extra large silicon company limited product; Defoamer Defom 6800 is a DEUCHEM company product; Aromatic alcohol phenylcarbinol or phenylethyl alcohol are the prosperous industrial corporation of Shanghai group product.The present invention is to be the hot construction structure glue of a kind of two-pack moisture-proof of base-material according to Resins, epoxy, and the raw material deal of first component and second component is wherein suitably adjusted, and can use under different temperature and wet environment.
Embodiment one
(1), the preparation of first component:
A. add endurable active toughener thiorubber JLY-1211 part and liquid-state epoxy resin E51100 part in the agitator by weight, normal temperature stirred 3~5 minutes for 700 rev/mins.
B. add 68000.3 parts of reactive thinner E-108 part, 6 parts of PGE and defoamer Defom more by weight successively, normal temperature stirs 3~5 minutes until mixing for 700 rev/mins.
C. add silane coupling agent KH5601 part by weight in the described liquid of step (1) b, stirring at normal temperature is even;
D. add 1 part of the white carbon black of hydrophobic gas phase by weight in the described liquid of step (1) c, stir, with 1400~2000 rev/mins of high-speed stirring 15 minutes, leave standstill froth breaking and promptly get the first component again until no visible meal;
(2), the preparation of second component
A. in the reaction vessel by weight with 90 parts of IPDA, 10 parts of MXDA, left standstill after mixing 10 minutes;
B. add 80 parts of phenylcarbinols, 7 parts of Whitfield's ointments more by weight successively, stir and mixed in 30 minutes, drip step (2) a gained liquid again, dropwise in one and a half hours;
C. add 15 parts of Resins, epoxy E44 by weight in step (2) the b gained liquid, keep temperature to mix half an hour below 40 ℃, get second component solidifying agent;
D. 1 part of altax P-30 is joined in 50 parts of described second component solidifying agent by weight, stirred 10 minutes, promptly get the second component.
Above-mentioned first component for preparing and second component were mixed by weight 1.5: 1 to 3: 1, promptly get wet and heat ageing resistant construction structure glue of the present invention.
Embodiment two
Liquid-state epoxy resin E-51 changes 12880 parts in the first component of embodiment one, the white carbon black of hydrophobic gas phase changes 2 parts into, and reactive thinner E-10 changes 6 parts into, and reactive thinner PGE changes 8 parts into, endurable active toughener thiorubber JLY-121 changes 0.6 part into, and silane coupling agent KH560 changes 1.5 parts into; Material and weight part change in the second component: 75 parts of IPDA, MXDA25 part, 70 parts of phenylethyl alcohols, 10 parts of Whitfield's ointments, 25 parts of epoxy resin E-44s.
The ratio of solidifying agent and altax P-30 weight part is 45: 2 in the second component.
All the other and preparation method are with embodiment one
Embodiment three
In the first component of embodiment one: liquid-state epoxy resin 128 changes 120 parts into, defoamer Defom 6800 changes 0.8 part into, and reactive thinner changes 7 parts of E10 into, 7 parts of PGE, endurable active toughener thiorubber JLY-121 changes 1.5 parts into, and silane coupling agent KH560 changes 2 parts into; Material and weight part change in the second component: 95 parts of IPDA, 5 parts of MXDA, 85 parts of phenylcarbinols, 12 parts of Whitfield's ointments, 25 parts of epoxy resin E-44s.The ratio of altax P-30 and solidifying agent is 3: 80 in the second component.
All the other and preparation method are with embodiment one.
Embodiment one, two, three and performance test data domestic, external like product
Actual items Physical condition External product Home products Embodiment one Embodiment two Embodiment three
Tensile strength (MPA) Normal temperature 7 days 41.5 36.9 18.4 16.5 45.8
Tensile modulus (MPA) Normal temperature 7 days 2.8×10 3 1.89×10 3 3.01×10 3 3.21×10 3 2.95×10 3
Rate (MPA) is stretched in fracture Normal temperature 7 days 1.8 1.9 2.5 2.4 3.1
Compressive strength (MPA) Normal temperature 7 days 106.0 93.0 101.5 105.6 99.0
Flexural strength (MPA) Normal temperature 7 days 77.6 45.0 73.4 74.5 76.9
Tensile shear strength (MPA) Normal temperature 7 days 16.7 17.4 19.8 20.2 21.1
Cloth and concrete bonding intensity (MPA) Normal temperature 3 days Concrete destruction Concrete destruction Concrete destruction Concrete destruction Concrete destruction
The artificial wet and heat ageing resistant shearing resistance (MPA) of quickening 50 ℃ of temperature relative humidity 98%90 days 15.1 14.9 18.6 19.5 19.8
Thermal distortion (℃) 60 ℃ of normal temperature 7 days 2 hours 53.2 45.2 55.3 53.9 56.4
Above performance test data is provided by electronic universal experimental machine (CMP-6504) test.
The present invention carries out performance test artificial the acceleration under the wet and heat ageing resistant condition (50 ℃, relative humidity 98%, 90 day), and shearing resistance descends all in 10% scope, and shearing resistance is higher, has high cost performance, meets national A level glue standard.The home products shearing resistance descends and surpasses 10%, does not meet national A level glue standard, the construction reinforcement restricted application.

Claims (5)

1. dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive is made of the first and second two kinds of components, and synthesis technique is:
(1) preparation of first component
A. add 0.5~2 part of endurable active toughener thiorubber, 75~120 parts of liquid-state epoxy resins in the agitator by weight, stirring at normal temperature is even;
B. add reactive thinner C more by weight 12-140.1~1 part of 6~8 parts of tertiary carbonic acid glycidyl esters, 6~8 parts of reactive thinner phenyl glycidyl ethers and defoamer, stirring at normal temperature is even;
C. add 0.5~2 part of silane coupling agent by weight in the described liquid of step (1) b, stirring at normal temperature is even;
D. add 1~2 part of the white carbon black of hydrophobic gas phase by weight in the described liquid of step (1) c, stir,, leave standstill froth breaking and promptly get the first component after 15 minutes with 1400~2000 rev/mins of high-speed stirring again;
(2) preparation of second component
A. in the reaction vessel by weight with 70~95 parts of isophorone diamines, 5~30 parts of m-xylene diamines, left standstill after mixing 10 minutes;
B. add 60~90 parts of aromatic alcohols, 5~15 parts of catalyzer Whitfield's ointments more by weight successively, mix, be added dropwise to step (2) a gained liquid, dropwise in one and a half hours;
Add 10~30 parts of Resins, epoxy E44 by weight in c step (2) the b gained liquid, keep temperature to mix half an hour below 40 ℃, get second component solidifying agent;
D. by weight 1~3 part of promotor is joined in 40~80 parts in the described second component solidifying agent, stirred 10 minutes, promptly get the second component.
2. a kind of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive according to claim 1 is characterized in that: described first component and the matching used weight proportion of described second component are 1.5: 1 to 3: 1.
3. a kind of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive according to claim 1 is characterized in that: described aromatic alcohol is a phenylcarbinol, or is phenylethyl alcohol.
4. a kind of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive according to claim 1 is characterized in that: described defoamer is Defom 6800.
5. a kind of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive according to claim 1 is characterized in that: described promotor is DMP-30.
CNA2007100377332A 2007-02-28 2007-02-28 Synthesis technique of dual-component wet and heat ageing resistant epoxy building structure strengthening adhesive Pending CN101255325A (en)